Free-cutting high-strength tellurium-copper alloy and preparation method and application thereof
By adding rare earth elements to tellurium copper alloy and adopting the upper-induction continuous casting process, the problem of low Zr solubility in the prior art is solved, the conductivity and tensile strength of tellurium copper alloy are improved, and easy cutting, high conductivity and High temperature resistance, suitable for charging pile connectors, reducing preparation costs and cycles.
Patent Information
- Application Number
- CN202411057385.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-02
- Publication Date
- 2024-11-19
AI Technical Summary
During the preparation process of existing tellurium copper alloys, the solubility of Zr is relatively low, which affects thermal stability and conductivity. The number of annealings often increases the preparation cycle and cost, which cannot meet the simultaneous requirements of high strength and high conductivity.
By adding rare earth elements La, Bi, Hf, and Ag to the tellurium copper alloy, the content of the alloy element and the initial grain structure are adjusted, and the final grain structure and texture are adjusted by using the upper-induction continuous casting, extrusion, drawing and annealing processes. Type, improves the easy cutting, high conductivity and high temperature resistance of materials.
It realizes efficient and low-cost copper tellurium alloy preparation, with high electrical conductivity, improved tensile strength, excellent cutting performance, suitable for charging pile connectors, extending the service life of the material.
Smart Images

Figure CN118979174A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal materials, and in particular to an easy-to-cut high-strength tellurium-copper alloy and a preparation method and application thereof. Background Art
[0002] With the continuous development of the global economy, people's consumption capacity has gradually increased, and the demand in the automobile market has also increased. As an emerging force, new energy vehicles are gradually integrating into people's daily lives and occupying an increasingly significant share in the total number of vehicles. In order to support the rapid development of the new energy vehicle industry, it is particularly important to build a sufficient number of charging facilities. Charging piles are as important to electric vehicles as traditional cars rely on gas stations. They can ensure that electric vehicles have a continuous supply of electricity. Charging piles are easy to install and can be conveniently deployed on the ground, walls, parking lots or dedicated charging stations. According to the endurance requirements of electric vehicles, they can be connected to AC power of the corresponding voltage level. Just align the charging plug with the charging port of the vehicle and insert it to start the continuous charging process.
[0003] The connector conductor in the charging pile is made by turning process, and its surface smoothness mainly depends on the quality of turning process, which is closely related to the cutting performance of the conductor. When the plug of the charging pile is connected to the socket, the contact surface is not completely smooth. Through high-power magnifying glass observation, it can be found that the contact surface is actually composed of many tiny bumps and bumps, which means that the actual contact is achieved through these tiny protruding points. When the current passes through the contact surface, it is not evenly distributed like an ideal plane, but concentrated on these contact points, resulting in a significant reduction in the actual contact area, the current shrinks at these points, and the resistance increases accordingly. The increase in resistance will cause more Joule heat to be generated when the current passes, which will increase the temperature of the metal part of the contact surface, which may affect its performance. Therefore, there are very strict requirements for the cutting accuracy of the material. At the same time, the conductive performance of the material is also crucial, because the connector will generate Joule heat during the power-on process, which will lead to energy loss.
[0004] The connector materials used for plugs and sockets are generally copper alloys. Currently, the materials used to make charging pile connectors are mainly red copper, brass, and high-copper alloys such as Sn-Cu, Mg-Cu and Ag-Cu. The main strategy to improve the cutting performance of connectors made of such high-copper alloy materials as Sn-Cu, Mg-Cu and Ag-Cu is to enhance the hardness of highly conductive materials. However, such materials are not suitable for precision connectors.
[0005] As the application of tellurium in copper materials has attracted the attention of the industry, related research has gradually increased. According to the research of Song Mingzhao and others, trace tellurium (Te) has little effect on the conductivity of pure copper, and its conductivity is similar to that of copper. At the same time, it can significantly improve the arc erosion resistance and cutting performance of copper materials. At present, developed countries such as Europe and the United States have conducted in-depth research and development on the excellent performance of tellurium copper alloys, and have developed a variety of products according to different application scenarios. In comparison, my country's research on tellurium copper alloys started late. Considering the huge consumption of copper alloys in my country and the strong demand for high-precision charging pile materials, the development of a tellurium copper alloy product suitable for high-current connection is of great significance to meet the needs of the rapid development of my country's charging pile industry.
[0006] Patent application number 202210772077.5 discloses a tellurium copper alloy and its preparation method. A tellurium copper alloy that is easy to turn, resistant to high temperature softening, has high conductivity, meets welding requirements and can be continuously produced is developed by adding S, Zr, and Sn to the tellurium copper alloy and controlling the amount of addition.
[0007] Patent application number 202310053303.9 discloses a tellurium copper alloy strip and its preparation method. In this scheme, a high-performance tellurium copper alloy material with high conductivity and good bending performance is prepared by smelting → semi-continuous casting → hot rolling → homogenization annealing → cold working → stress relief annealing, and its conductivity is ≥97% IACS and its tensile strength is ≥280MPa.
[0008] The above patent discloses a tellurium copper alloy and a preparation method thereof, which improves the tellurium copper performance by adding Zr to the tellurium copper alloy, but the solubility of Zr at the eutectic temperature is low, and the precipitation potential is small, which has a great impact on thermal stability and conductivity. The above patent discloses a tellurium copper alloy strip and a preparation method thereof, although the conductivity of the prepared product is high, its tensile strength is low. After two annealings, the conductivity is increased by sacrificing the tensile strength, which reduces the product's load-bearing capacity and cannot meet the requirements of some special customers. In addition, the two annealings and semi-continuous casting not only increase the preparation cycle, but also increase the manufacturing cost. Summary of the invention
[0009] In order to solve the above technical problems, the present invention provides a tellurium copper alloy with high strength and easy cutting, and its preparation method and application. Through upward continuous casting, rare earth elements La, Bi, Hf, and Ag are added to adjust the alloy element content and initial grain structure, and through extrusion, drawing, and annealing, the final grain structure and texture type and content are adjusted to finally achieve the characteristics of easy cutting, high conductivity, and high temperature resistance.
[0010] The present invention is achieved through the following technical solutions:
[0011] The first object of the present invention is to provide a free-cutting high-strength tellurium-copper alloy. The constituent elements of the free-cutting high-strength tellurium-copper alloy include, by mass percentage, Te: 0.056%-0.095%, La: 0.027%-0.066%, Bi: 0.152%-0.193%, Hf: 0.254%-0.344%, Ag: 0.035%-0.097%, and the rest are Cu and unavoidable impurities.
[0012] In one embodiment of the present invention, the Te is added as a raw material in the form of a tellurium-copper master alloy; the content of Te in the tellurium-copper master alloy is 55wt%-65wt%.
[0013] In one embodiment of the present invention, the Bi and Ag are both in the form of single metals, wrapped in copper foil and added as raw materials.
[0014] In one embodiment of the present invention, the La is added as a raw material in the form of a copper-lanthanum master alloy, and the content of La in the copper-lanthanum master alloy is 8wt%-12wt%.
[0015] In one embodiment of the present invention, the Hf is added as a raw material in the form of a copper-hafnium master alloy, and the content of Hf in the copper-hafnium master alloy is 7wt%-9wt%.
[0016] The second object of the present invention is to provide a method for preparing the free-cutting high-strength tellurium-copper alloy, comprising the following steps:
[0017] (1) adding high-purity cathode copper to the melting furnace in the upper furnace, the melting temperature is 1140°C-1200°C, covering the transition chamber and the melting furnace surface with dried charcoal to protect the melt, and covering the surface of the holding furnace with graphite flakes to protect the melt;
[0018] (2) adding the raw materials into a melting furnace in the form of single metal or master alloy and performing electromagnetic stirring;
[0019] (3) The crystallizer is lowered to 40 mm below the liquid level and upward casting is started to produce continuous alloy rods with a diameter of 20 mm;
[0020] (4) continuously extruding the upper lead rod to obtain an extruded rod with a specification of 16 mm;
[0021] (5) using a continuous cold rolling mill to roll the extruded billet into a bar with a diameter of 8 mm;
[0022] (6) The Ø8 mm rod obtained in step (5) is subjected to aging treatment, and a Ø3 mm tellurium copper alloy rod is obtained by drawing using a combined drawing machine.
[0023] In one embodiment of the present invention, in step (1), the thickness of the charcoal is 100 mm-140 mm;
[0024] And / or, the thickness of the graphite flakes is 120 mm-150 mm.
[0025] In one embodiment of the present invention, in step (3), the temperature of the upward casting is 1140°C-1200°C;
[0026] And / or, the upward casting speed is 300mm / min-350mm / min.
[0027] In one embodiment of the present invention, in step (4), the rotation speed of the extrusion wheel of the continuous extrusion is 6.0 rpm-7.2 rpm.
[0028] In one embodiment of the present invention, in step (6), the aging treatment is carried out at a temperature of 430° C. to 460° C. and for a time of 1 h to 3 h.
[0029] The third object of the present invention is to provide the use of the easy-to-cut high-strength tellurium copper alloy in the preparation of connector conductors for charging piles.
[0030] The reason for limiting the metal type and addition amount in the free-cutting high-strength tellurium-copper alloy material of the present invention is:
[0031] Tellurium: Tellurium is dispersed in the copper matrix as an independent phase Cu2Te, with good high temperature stability and easy chip breaking, thus improving the cutting performance, electrical conductivity and arc extinguishing performance of copper alloy materials. Trace tellurium significantly improves the electrical conductivity, arc resistance and cutting performance of copper, Te: 0.056%-0.095%, the best is 0.072%;
[0032] Bismuth: The addition of bismuth improves the quality of the material processing surface, reduces the surface roughness, and achieves the effect of easy cutting. In copper-bismuth alloys, when the bismuth content is in the range of 0.05%-0.152%, since bismuth is evenly distributed in the (α+β) phase in a point-like manner, it is difficult for copper chips to form a good fracture during the cutting process, and the copper chips present a slender spiral shape. At the same time, due to the long-term and large-area contact between the copper chips and the tool, the cutting resistance is increased, causing the tool to easily heat up and the color of the copper chips to darken. However, when the bismuth content is increased to 0.152%-0.193%, the copper chips become smaller and needle-shaped, evenly distributed and loose. This is because as the bismuth content increases, the number of evenly distributed bismuth points in the (α+β) phase increases, and the number of bismuth particles on the grain boundary between the (α+β) phase and the β phase also increases, which reduces the cutting resistance and increases the fracture source of the copper chips, thereby improving the cutting performance of the bismuth-containing copper alloy. The bismuth content is preferably 0.152%-0.193%.
[0033] Lanthanum: When rare earth lanthanum is added to copper liquid, it helps to reduce the defects that may occur in pure copper during the casting process, and at the same time purifies the copper matrix and grain boundaries, achieving the effects of deoxidation, desulfurization, purification and grain refinement. These effects significantly improve the electrical conductivity, enhance its tensile strength, and significantly improve the hardness. In addition, in copper liquid, lanthanum combines with elements such as bismuth to form refractory binary or multi-metallic compounds with high hardness, such as BiLa. These compounds with high melting points are dispersed and suspended in the melt in the form of tiny particles, acting as dispersed crystallization cores, promoting the increase of pure copper grain boundaries and the refinement of grains. Refined grains increase the resistance to dislocation movement and shorten the length of dislocation accumulation groups inside the grains, thereby improving the yield strength and tensile strength of the material. The lanthanum content is preferably 0.027%-0.066%, and the best is 0.041%. The comprehensive performance at this ratio reaches the best state.
[0034] Silver: A trace amount of silver does not significantly reduce the electrical conductivity and thermal conductivity of copper, and can significantly increase the recrystallization temperature, creep resistance and wear resistance. The silver content is preferably 0.035%-0.097%.
[0035] Hafnium: The properties of hafnium are very similar to those of its coexisting Zr. Adding Hf elements to copper alloys can also increase thermal stability through the aging process and inhibit grain growth. The degree of thermal stability enhancement is higher than that of Zr, because the solubility of Hf at the eutectic temperature is 0.3at%, which is much larger than that of Zr. In addition, Hf has great precipitation strengthening potential. The precipitated fine Hf phase can pin dislocations and hinder dislocation movement, thereby increasing strength. At the same time, the recovery of lattice distortion weakens the scattering effect of electrons and improves conductivity.
[0036] The above technical solution of the present invention has the following advantages compared with the prior art:
[0037] (1) Compared with the traditional "three-stage" process, the short process "upward continuous casting + continuous extrusion" mentioned in the present invention has the characteristics of short manufacturing process, low investment, high efficiency and energy saving, reduced cost, dense product structure, fine grains, good mechanical properties and conductive properties, and can realize large-scale continuous production.
[0038] (2) The addition of trace alloying elements can effectively purify the melt, refine the grains, and make the alloy structure uniform and dense, which not only improves the overall performance, but also helps to reduce casting defects, thereby ensuring that the alloy material has excellent electrical conductivity, mechanical properties, resistance to high temperature softening, and easy cutting properties.
[0039] (3) The present invention can be well applied to connectors in charging piles, and has excellent tensile strength, electrical conductivity, cutting performance, high temperature resistance, etc., which is beneficial to improving the service life of the material. BRIEF DESCRIPTION OF THE DRAWINGS
[0040] In order to make the content of the present invention more clearly understood, the present invention is further described in detail below according to specific embodiments of the present invention in conjunction with the accompanying drawings, wherein:
[0041] Figure 1 This is a diagram showing the cutting debris of the tellurium copper alloy prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0042] The present invention is further described below in conjunction with the accompanying drawings and specific embodiments so that those skilled in the art can better understand the present invention and implement it, but the embodiments are not intended to limit the present invention.
[0043] The invention provides a free-cutting high-strength tellurium copper alloy. The free-cutting high-strength tellurium copper alloy comprises the following elements and mass percentages: Te: 0.056%-0.095%, La: 0.027%-0.066%, Bi: 0.152%-0.193%, Hf: 0.254%-0.344%, Ag: 0.035%-0.097%, and the rest is Cu and unavoidable impurities.
[0044] The electrical conductivity of the easy-to-cut, high-strength, high-conductivity, high-temperature-resistant tellurium copper is ≥92% IACS, the softening temperature is ≥550° C., the tensile strength is ≥600 MPa, and the chipping performance is excellent.
[0045] The method for preparing the free-cutting high-strength tellurium copper alloy comprises the following steps:
[0046] (1) Upward continuous casting: Add high-purity cathode copper to the melting furnace, add it to the melting furnace according to the above alloy element ratio and perform electromagnetic stirring, stir it evenly, and then flow it into the transition bin and the insulation furnace from the melting furnace. The insulation furnace is covered with graphite flakes with a thickness of about 120mm-150mm, and the transition bin and the insulation furnace are covered with dried charcoal with a thickness of about 100mm-140mm. Use a crystallizer to insert the copper liquid to a certain depth to start upward casting, control the casting temperature at 1140℃-1200℃, and control the upward speed at 300mm / min-350mm / min to prepare a continuous Ф20mm alloy rod;
[0047] (2) Continuous extrusion: In the continuous extrusion process, the heat generated by the alloy material during the deformation process may be as high as 600 to 700°C, resulting in a significant increase in the temperature of the extruded rod. In order to effectively reduce the temperature, a water cooling system is used to quickly cool the metal rod flowing out of the extrusion die hole. Subsequently, the wire is wound through a tension winding mechanism. The optimal speed of the extrusion wheel is 6.0rpm-7.2rpm;
[0048] (3) Cold rolling: Use a continuous cold rolling mill to roll the extruded billet to Ø8 mm;
[0049] (4) Aging: The aging treatment temperature is 430℃~460℃, and the aging time is 1h~3h;
[0050] (5) Drawing: After aging, use a combined drawing machine to draw the steel to Ф3mm.
[0051] Furthermore, the Te in the alloy material in step (1) is added as a raw material in the form of a tellurium-copper master alloy, and the content of Te in the tellurium-copper master alloy is 60 wt %;
[0052] Furthermore, the Bi and Ag in the alloy material of step (1) are both in the form of single metals, wrapped in copper foil and added as raw materials;
[0053] Furthermore, the La in the alloy material of step (1) is added as a raw material in the form of a copper-lanthanum master alloy, and the La content in the copper-lanthanum master alloy is 10 wt %;
[0054] Furthermore, the Hf in the alloy material of step (1) is added as a raw material in the form of a copper-hafnium master alloy, and the content of Hf in the copper-hafnium master alloy is 8 wt %;
[0055] Furthermore, in step (1), electromagnetic stirring is to promote the mixing of the copper liquid by applying electromagnetic force to ensure uniform distribution of components, thereby forming a high-quality solidification structure to obtain an excellent rod blank;
[0056] Furthermore, in the casting of step (1), the crystallizer needs to be 40 mm below the liquid surface;
[0057] Furthermore, the continuous extrusion in step (2) has an extrusion specification of Φ16 mm;
[0058] Furthermore, in step (3), the cold rolling is performed four times;
[0059] Furthermore, in step (4), the aging treatment temperature is 450° C. and the aging time is 2 h;
[0060] The cutting performance was tested on a lathe under the process conditions of a lathe speed of 1000 r / min, a tool feed depth of 0.5 mm and a tool feed amount of 0.16 mm.
[0061] Example 1
[0062] The present embodiment provides a free-cutting high-strength tellurium-copper alloy and a preparation method thereof. The components and mass percentages of the tellurium-copper alloy are: Te: 0.072wt%, Ag: 0.049wt%, Bi: 0.178wt%, Hf: 0.309wt%, La: 0.041wt%, and the rest are Cu and unavoidable impurities.
[0063] The method for preparing the free-cutting high-strength tellurium-copper alloy based on the above composition in this embodiment comprises the following steps:
[0064] Step 1: Add high-purity cathode copper to the melting furnace in the upper furnace, the melting temperature is 1172°C, the transition chamber and the melting furnace are covered with dried charcoal to protect the melt, the thickness is about 123mm, and the surface of the insulation furnace is covered with graphite flakes to protect the melt, the thickness is about 133mm;
[0065] Step 2: First add the Cu-60wt%Te master alloy wrapped in copper foil until it is completely melted, the melting temperature is 1172°C, then add the Bi and Ag metal elements wrapped in copper foil in sequence, and then add the Cu-8wt%Hf and Cu-10wt%La master alloys wrapped in copper foil until they are melted, the melting temperature is 1172°C, and electromagnetic stirring is performed at the same time;
[0066] Step 3: The crystallizer is lowered to 40 mm below the liquid surface, and upward casting is started. The casting temperature is controlled at about 1170°C, and the upward speed is controlled at 330 mm / min to prepare continuous 20 mm Ø alloy rods.
[0067] Step 4: preheat the extrusion tooling die to 600°C for 2 hours, and continuously extrude the upper lead rod to obtain an extruded rod with a specification of Ф16mm. The extrusion wheel speed is 6.5rpm;
[0068] Step 5: Use a continuous cold rolling mill to roll the extruded billet from 16mm to 14mm to 12mm to 10mm to 8mm;
[0069] Step 6: Aging the Ø8mm bar that has been cold rolled in step 5 at a temperature of 450°C for 2 hours;
[0070] Step 7: Use a combined drawing machine to draw the rod into a 3mm diameter bar;
[0071] The final product of the present invention has the following properties: conductivity 93.4% IACS, high temperature softening temperature 567°C, and tensile strength 613MPa. Referring to the nonferrous industry standard YS / T648-2007, the finished product prepared in this embodiment has excellent chip performance, which is category 1, and the chips are granular and the cutting presents spiral curly short thin strips (the chip situation is as follows Figure 1 shown).
[0072] Example 2
[0073] The present embodiment provides a free-cutting high-strength tellurium-copper alloy and a preparation method thereof. The components and mass percentages of the tellurium-copper alloy are: Te: 0.056wt%, Ag: 0.035wt%, Bi: 0.193wt%, Hf: 0.254wt%, La: 0.066wt%, and the rest are Cu and unavoidable impurities.
[0074] The preparation method of the free-cutting, high-strength, high-conductivity, high-temperature-resistant tellurium-copper alloy based on the above composition in this embodiment is the same as that in Example 1.
[0075] The final product obtained by the present invention has the following properties: electrical conductivity 93.1% IACS, high temperature softening temperature 569°C, tensile strength 620MPa, cutting to present spirally curled short thin strips, and excellent cutting performance.
[0076] Example 3
[0077] The present embodiment provides a free-cutting high-strength tellurium-copper alloy and a preparation method thereof. The components and mass percentages of the tellurium-copper alloy are: Te: 0.095wt%, Ag: 0.097wt%, Bi: 0.152wt%, Hf: 0.344wt%, La: 0.027wt%, and the rest are Cu and unavoidable impurities.
[0078] The preparation method of the free-cutting, high-strength, high-conductivity, high-temperature-resistant tellurium-copper alloy based on the above composition in this embodiment is the same as that in Example 1.
[0079] The final product of the present invention has the following properties: conductivity 94.8% IACS, high temperature softening temperature 558°C, tensile strength 609MPa, cutting presents spiral curled short thin strips, and excellent cutting performance (refer to nonferrous industry standard YS / T648-2007)
[0080] Comparative Example 1
[0081] The present embodiment provides a free-cutting high-strength tellurium-copper alloy and a preparation method thereof. The components and mass percentages of the tellurium-copper alloy are: Te: 0.072wt%, Ag: 0.049wt%, Bi: 0.178wt%, Hf: 0.309wt%, and the rest are Cu and unavoidable impurities.
[0082] The final product performance of this comparative example is: conductivity 84.2% IACS, high temperature softening temperature 516°C, tensile strength 536MPa, cutting shows spiral curling short thin strips, poor cutting performance, belonging to category 3 (refer to non-ferrous industry standard YS / T648-2007)
[0083] Comparative Example 2
[0084] The present embodiment provides a free-cutting high-strength tellurium-copper alloy and a preparation method thereof. The components and mass percentages of the tellurium-copper alloy are: Te: 0.072wt%, Ag: 0.049wt%, Bi: 0.178wt%, La: 0.041wt%, and the rest are Cu and unavoidable impurities.
[0085] The final product performance of this comparative example is: conductivity 86.2% IACS, high temperature softening temperature 487℃, tensile strength 561MPa, the debris is a random spiral curling winding form, but it does not affect the speed and surface finish, the cutting performance is poor, belonging to category 2 (refer to the non-ferrous industry standard YS / T648-2007)
[0086] Obviously, the above embodiments are merely examples for clear explanation and are not intended to limit the implementation methods. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the implementation methods here. The obvious changes or modifications derived from these are still within the protection scope of the invention.
Claims
1. A free-cutting high-strength tellurium copper alloy, characterized in that: Measured by mass percentage, the constituent elements of the free-cutting high-strength tellurium copper alloy include: Te: 0.056%-0.095%, La: 0.027%-0.066%, Bi: 0.152%-0.193%, Hf: 0.254%-0.344%, Ag: 0.035%-0.097%, and the rest are Cu and unavoidable impurities.
2. The tellurium copper alloy according to claim 1, characterized in that: The Te is added as a raw material in the form of a tellurium-copper master alloy; the content of Te in the tellurium-copper master alloy is 55wt%-65wt%.
3. The tellurium copper alloy according to claim 1, characterized in that: The Bi and Ag are both in the form of single metals, wrapped in copper foil and added as raw materials.
4. The tellurium copper alloy according to claim 1, characterized in that: The La is added as a raw material in the form of a copper-lanthanum master alloy, and the content of La in the copper-lanthanum master alloy is 8wt%-12wt%.
5. The tellurium copper alloy according to claim 1, characterized in that: The Hf is added as a raw material in the form of a copper-hafnium master alloy, and the content of Hf in the copper-hafnium master alloy is 7wt%-9wt%.
6. The method for preparing the free-cutting high-strength tellurium-copper alloy according to any one of claims 1 to 5, characterized in that: The following steps are involved: (1) adding high-purity cathode copper to the melting furnace in the upper furnace, the melting temperature is 1140°C-1200°C, covering the transition chamber and the melting furnace surface with dried charcoal to protect the melt, and covering the surface of the holding furnace with graphite flakes to protect the melt; (2) adding the raw materials into a melting furnace in the form of single metal or master alloy and performing electromagnetic stirring; (3) The crystallizer is lowered to 40 mm below the liquid level and upward casting is started to produce continuous alloy rods with a diameter of 20 mm; (4) continuously extruding the upper lead rod to obtain an extruded rod with a specification of 16 mm; (5) using a continuous cold rolling mill to roll the extruded billet into a bar with a diameter of 8 mm; (6) The Ø8 mm rod obtained in step (5) is subjected to aging treatment, and a Ø3 mm tellurium copper alloy rod is obtained by drawing using a combined drawing machine.
7. The preparation method according to claim 6, characterized in that: In step (3), the temperature of the upward casting is 1140° C.-1200° C.; And / or, the upward casting speed is 300mm / min-350mm / min.
8. The preparation method according to claim 6, characterized in that: In step (4), the rotation speed of the extrusion wheel of the continuous extrusion is 6.0 rpm-7.2 rpm.
9. The preparation method according to claim 6, characterized in that: In step (6), the temperature of the aging treatment is 430° C. to 460° C., and the time is 1 h to 3 h.
10. Use of the easy-to-cut high-strength tellurium copper alloy according to any one of claims 1 to 5 in preparing connector conductors for charging piles.