Silicon-doped diamond-like composite lubricating coating as well as preparation method and application thereof

By introducing a dual-layer structure of SiC base layer and Si-DLC functional layer into the DLC coating, combining DC magnetron sputtering and anode ion source assisted high-power pulse magnetron sputtering technology, the traditional DLC coating is solved in flexibility The problem of easy peeling on the substrate has achieved a silicon-doped diamond-like composite lubricating coating with high hardness, high toughness and crack resistance. It is suitable for a variety of substrates and exhibits excellent lubricating effects at high temperatures.

CN118979220AActive Publication Date: 2024-11-19GUANGDONG INST OF NEW MATERIALS
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411076802.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-19
Estimated Expiration
2044-08-07

AI Technical Summary

Technical Problem

Traditional DLC coatings are easy to peel off when applied on flexible substrates, and have poor toughness and high internal stress, making it difficult to achieve high hardness, high toughness and crack resistance at the same time.

Method used

Using the dual-layer structure of SiC base layer and Si-DLC functional layer, silicon-doped diamond composite lubricating coating is prepared through DC magnetron sputtering and anode ion source assisted high-power pulse magnetron sputtering technology to optimize the coating Stressed state and microstructure improve their hardness and toughness.

Benefits of technology

It realizes the low friction, high hardness, high toughness and crack resistance of silicon-doped diamond composite lubricating coating. It is suitable for hard and flexible substrates, broadens its application range, and has excellent lubrication and friction reduction in high temperature environments. Effect.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118979220A_ABST
    Figure CN118979220A_ABST
Patent Text Reader

Abstract

The invention discloses a silicon-doped diamond-like composite lubricating coating as well as a preparation method and application thereof, and belongs to the technical field of wear-resistant coatings. The silicon-doped diamond-like carbon composite lubricating coating comprises a SiC base coat and a Si-DLC functional layer which are sequentially arranged on the surface of a substrate, wherein the SiC base coat is of a columnar structure, and the thickness of the SiC base coat ranges from 0.3 micrometer to 0.4 micrometer; the Si-DLC functional layer has a compact feature-free structure, and the thickness of the Si-DLC functional layer is 2.0 [mu] m-5. 0 [mu] m. The coating can have low friction, high hardness, high toughness, high wear resistance and cracking resistance at the same time. The preparation method is simple and easy to operate, and has the characteristics of low deposition temperature, uniform film formation, good repeatability, wide practicability and the like. The obtained coating can be used for a hard substrate and can also be used for a flexible substrate, and the application range of the diamond-like carbon film is greatly widened.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of wear-resistant coatings, and in particular to a silicon-doped diamond-like composite lubricating coating and a preparation method and application thereof. Background Art

[0002] In many cases, the surface of materials is susceptible to various damages such as scratches, wear and erosion, so it is necessary to prepare corresponding protective coatings on their surfaces. Among them, diamond-like carbon (DLC) coatings are widely used in the fields of machinery, electronics, medicine, etc. as protective coatings due to their low friction coefficient, high hardness, high wear resistance and chemical inertness. However, traditional DLC coatings have problems such as poor toughness and easy peeling of the coating due to large internal stress, especially when applied on flexible substrates, which easily leads to fracture.

[0003] Therefore, it is of great significance to prepare high-performance DLC lubricating coatings with high hardness, high toughness, high wear resistance and crack resistance.

[0004] In view of this, the present invention is proposed. Summary of the invention

[0005] The purpose of the present invention is to provide a silicon-doped diamond-like composite lubricating coating and a preparation method and application thereof.

[0006] The present invention can be implemented like this:

[0007] In a first aspect, the present invention provides a silicon-doped diamond-like composite lubricating coating, the silicon-doped diamond-like composite lubricating coating comprising a SiC primer layer and a Si-DLC functional layer sequentially disposed on a substrate surface;

[0008] The SiC base layer has a columnar structure, and the thickness of the SiC base layer is 0.3 μm to 0.4 μm; the Si-DLC functional layer has a dense featureless structure, and the thickness of the Si-DLC functional layer is 2.0 μm to 5.0 μm.

[0009] In an optional embodiment, in the SiC base layer, the mass percentage of Si is 25% to 35%, and the mass percentage of C is 65% to 75%.

[0010] In an optional embodiment, in the Si-DLC functional layer, the mass percentage of Si is 2% to 8%, and the mass percentage of DLC is 92% to 98%.

[0011] In an optional embodiment, the silicon-doped diamond-like composite lubricating coating has at least one of the following characteristics:

[0012] Feature 1: The hardness of the silicon-doped diamond-like composite lubricating coating is H, and the range of H is 18 GPa to 25 GPa; preferably, H is 18.0 GPa to 24.6 GPa;

[0013] Feature 2: The equivalent elastic modulus of the silicon-doped diamond-like composite lubricating coating is E*, H / E*≥0.1; preferably, H / E* is 0.102-0.106;

[0014] Feature 3: The elastic recovery coefficient of the silicon-doped diamond-like composite lubricating coating is We, We ≥ 60%; preferably, We is 76.5% to 82.2%;

[0015] Feature 4: The silicon-doped diamond-like composite lubricating coating is in a compressive stress state as a whole; preferably, the SiC base layer is in a tensile stress state, and the Si-DLC functional layer is in a compressive stress state;

[0016] Feature 5: The microstructure of silicon-doped diamond-like composite lubricating coating is dense;

[0017] Feature 6: The friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment of 25°C is 0.07 to 0.08; preferably, the friction coefficient is 0.072 to 0.079;

[0018] Feature 7: The friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450° C. is 0.040 to 0.065; preferably, the friction coefficient is 0.040 to 0.063;

[0019] Feature 8: The wear rate of silicon-doped diamond-like composite lubricating coating in an atmospheric environment of 25°C does not exceed 10 -7 m 3 / N·m;

[0020] Feature 9: The wear rate of silicon-doped diamond-like composite lubricating coating in 450°C atmospheric environment does not exceed 10 -6 m 3 / N·m;

[0021] Feature 10: During the friction process, the silicon-doped diamond-like composite lubricating coating forms a complete amorphous carbon transfer film in situ at the friction pair.

[0022] In a second aspect, the present invention provides a method for preparing a silicon-doped diamond-like carbon composite lubricating coating as described in any of the aforementioned embodiments, comprising the following steps: sequentially disposing a SiC primer layer and a Si-DLC functional layer on the surface of a substrate.

[0023] In an optional embodiment, the SiC base layer is prepared by a DC magnetron sputtering method;

[0024] The preparation conditions of SiC base layer include: the vacuum degree in the equipment chamber is better than 1.0×10 -3 Pa, 50sccm~80sccm of argon is introduced into the equipment, and the gas pressure is maintained at 0.2Pa~0.3Pa; the substrate bias is -50V~-100V, and the bias duty cycle is 50%~60%; the target current is 1.0A~2.0A, and the deposition time is 20min~30min.

[0025] In an optional embodiment, the target material is a graphite-silicon composite target, wherein the Si content accounts for 35wt% to 45wt%.

[0026] In an optional embodiment, the Si-DLC functional layer is prepared by high-power pulsed magnetron sputtering technology assisted by an anode ion source;

[0027] The preparation conditions of the Si-DLC functional layer include: the argon gas flow rate is 50sccm~80sccm, and the gas pressure is 0.2Pa~0.3Pa; the substrate bias is -50V~-100V, and the bias duty cycle is 50%~60%; a C-Si composite target is used, the Si content accounts for 5wt%~10wt%, the HiPIMS pulse power is 5.0kW~8.0kW, and the duty cycle is 1.0%~5.0%; the anode layer ion source assists the ionization of the sputtering gas, and the corresponding anode layer ion source power is 0.50kW~0.75kW, and the duty cycle is 50%~60%; the deposition time is 6h~10h.

[0028] In an optional embodiment, before preparing the SiC base layer, the substrate is also pre-treated.

[0029] In an optional embodiment, the pretreatment includes grinding and polishing the substrate, and then performing ultrasonic cleaning, and then placing the obtained substrate on a rotating rack in a vacuum chamber and performing plasma glow cleaning using an anode layer ion source.

[0030] In an optional embodiment, the ultrasonic cleaning time is 40 min to 50 min.

[0031] In an optional embodiment, the plasma glow cleaning includes: placing the substrate in a vacuum chamber, evacuating the vacuum to a value better than 1.0×10 -3 Pa, then introduce 100sccm~150sccm argon gas, and adjust the gas pressure to 0.36Pa~0.52Pa; at the same time, adjust the substrate bias to -1000V~-1200V, and the bias duty cycle is 50%~60%; then turn on the anode layer ion source, the anode layer ion source power is 0.8kW~1.0kW, the duty cycle is 50%~60%, and the plasma glow cleaning time is 30min~40min.

[0032] In a third aspect, the present invention provides an application of a silicon-doped diamond-like composite lubricating coating as described in any of the aforementioned embodiments. For example, the silicon-doped diamond-like composite lubricating coating can be used to be disposed on a hard substrate or a flexible substrate in the mechanical, electronic, or medical fields.

[0033] In alternative embodiments, the hard substrate comprises stainless steel or cemented carbide.

[0034] In alternative embodiments, the flexible substrate comprises a polymer, a metal foil, a flexible thin glass, or a textile.

[0035] The beneficial effects of the present invention include:

[0036] The present invention provides a SiC base layer and a Si-DLC functional layer with a specific thickness and structure on the surface of a substrate to obtain a silicon-doped diamond-like composite lubricating coating, so that the silicon-doped diamond-like composite lubricating coating has low friction, high hardness, high toughness, high wear resistance and crack resistance. The preparation method of the silicon-doped diamond-like composite lubricating coating is simple and easy to operate, and has the characteristics of low deposition temperature, uniform film formation, good repeatability and wide practicality. The obtained coating can be used for both hard substrates and flexible substrates, which greatly broadens the application range of diamond-like films. BRIEF DESCRIPTION OF THE DRAWINGS

[0037] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0038] Figure 1 This is a scanning electron microscope photograph of the cross section of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1;

[0039] Figure 2 The load-displacement curve of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1;

[0040] Figure 3 Actual photos of the high-strength, tough, and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1 after bending tests at different angles and the optical morphology photos of the corresponding crease surfaces;

[0041] Figure 4 This is the friction coefficient curve of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1 at room temperature (25°C) and 450°C high temperature atmosphere. DETAILED DESCRIPTION

[0042] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0043] The silicon-doped diamond-like composite lubricating coating provided by the present invention and its preparation method and application are described in detail below.

[0044] The invention provides a silicon-doped diamond-like composite lubricating coating. The silicon-doped diamond-like composite lubricating coating comprises a SiC primer layer and a Si-DLC functional layer which are sequentially arranged on the surface of a substrate.

[0045] The SiC base layer has a columnar structure, which can be clearly observed.

[0046] In an optional embodiment, in the SiC base layer, the mass percentage of Si is 25% to 35% (such as 25%, 28%, 30%, 32% or 35%, etc.), and the mass percentage of C is 65% to 75% (such as 65%, 68%, 70%, 72% or 75%, etc.).

[0047] The thickness of the SiC primer layer may be 0.3 μm to 0.4 μm, such as 0.3 μm, 0.35 μm or 0.4 μm, or may be other values ​​within the range of 0.3 μm to 0.4 μm.

[0048] If the SiC base layer is thin, it is not conducive to forming good adhesion between the Si-DLC functional layer and the SiC base layer; if the SiC base layer is thick, it is not conducive to the performance of the Si-DLC functional layer.

[0049] The Si-DLC functional layer has a dense featureless structure, where the above-mentioned “dense” may be understood as a porosity of no more than 1%.

[0050] In an optional embodiment, in the Si-DLC functional layer, the mass percentage of Si is 2% to 8% (such as 2%, 3%, 4%, 5%, 6%, 7% or 8%, etc.), and the mass percentage of DLC is 92% to 98% (such as 92%, 93%, 94%, 95%, 96%, 97% or 98%, etc.).

[0051] The thickness of the Si-DLC functional layer may be 2.0 μm to 5.0 μm, such as 2.0 μm, 2.5 μm, 3.0 μm, 3.5 μm, 4.0 μm, 4.5 μm or 5.0 μm, or any other value within the range of 2.0 μm to 5.0 μm.

[0052] If the thickness of the Si-DLC functional layer is too thin, it is not conducive to the performance of the Si-DLC functional layer; if the thickness of the Si-DLC functional layer is too thick, it is not conducive to the use of the Si-DLC functional layer in certain specific application scenarios.

[0053] In some embodiments, the hardness of the silicon-doped diamond-like composite lubricating coating is H, and H ranges from 18 GPa to 25 GPa. In some preferred embodiments, H is 18.0 GPa to 24.6 GPa, such as 20.6 GPa, 21.3 GPa, 19.4 GPa, 18.4 GPa, 19.8 GPa, 19.4 GPa, 21.5 GPa, 23.3 GPa, 20.3 GPa, 24.1 GPa, 18.0 GPa, 24.6 GPa, 21.5 GPa or 19.6 GPa, etc., and may also be other values ​​within the range of 18.0 GPa to 24.6 GPa.

[0054] In some embodiments, the equivalent elastic modulus of the silicon-doped diamond-like composite lubricating coating is E*, H / E*≥0.1. In some preferred embodiments, H / E* is 0.102-0.106, such as 0.101, 0.102, 0.103, 0.104, 0.105 or 0.106, and may also be other values ​​within the range of 0.102-0.106.

[0055] The above E*=E / (1-ν 2 ), where E is the elastic modulus and ν is the Poisson's ratio.

[0056] In some embodiments, the elastic recovery coefficient of the silicon-doped diamond-like composite lubricating coating is We, We ≥ 60%. In some preferred embodiments, We is 76.5% to 82.2%, such as 76.5%, 77.3%, 78.2%, 78.7%, 79.1%, 80.1%, 80.2%, 81.2% or 82.2%, and may be other values ​​within the range of 76.5% to 82.2%.

[0057] In some embodiments, the silicon-doped diamond-like composite lubricating coating is in a compressive stress state (σ<0) as a whole, wherein the SiC base layer is in a tensile stress state, and the Si-DLC functional layer is in a compressive stress state. The microstructure of the silicon-doped diamond-like composite lubricating coating is dense.

[0058] In some embodiments, the friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment of 25° C. is 0.07 to 0.08. In some preferred embodiments, the friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment of 25° C. is 0.072 to 0.079, such as 0.072, 0.073, 0.075, 0.076, 0.077, 0.078 or 0.079, etc., and may also be other values ​​within the range of 0.072 to 0.079.

[0059] In some embodiments, the friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450° C. is 0.040 to 0.065. In some preferred embodiments, the friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450° C. is 0.040 to 0.063, such as 0.040, 0.042, 0.047, 0.046, 0.049, 0.063, 0.058 or 0.041, etc., and may also be other values ​​within the range of 0.040 to 0.063.

[0060] In some embodiments, the wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 25° C. is no more than 10 -7 m 3 / N·m. In some preferred embodiments, the wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 25°C is 2.06×10 -7 m 3 / N·m~3.47×10 -7 m 3 / N·m, such as 2.06×10 -7 m 3 / N·m, 2.14×10 - 7 m 3 / N·m, 2.18×10 -7 m 3 / N·m, 2.33×10 -7 m 3 / N·m, 2.45×10 -7 m 3 / N·m,2.91×10 -7 m 3 / N·m、3.21×10 -7 m 3 / N·m、3.41×10 -7 m 3 / N·m,3.46×10 -7 m 3 / N·m or 3.47×10 -7 m 3 / N·m, etc., or 2.06×10-7 m 3 / N·m~3.47×10 -7 m 3 / Other values ​​within the range of N·m.

[0061] In some embodiments, the wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450° C. is no more than 10 -6 m 3 / N·m. In some preferred embodiments, the wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450°C is 1.33×10 -6 m 3 / N·m~4.45×10 -6 m 3 / N·m, such as 1.33×10 -6 m 3 / N·m,1.61×10 -6 m 3 / N·m,1.85×10 -6 m 3 / N·m,2.51×10 -6 m 3 / N·m,2.94×10 -6 m 3 / N·m,3.29×10 -6 m 3 / N·m,3.51×10 -6 m 3 / N·m,3.67×10 -6 m 3 / N·m,4.11×10 -6 m 3 / N·m,4.45×10 -6 m 3 / N·m, etc., or 1.33×10 -6 m 3 / N·m~4.45×10 -6 m 3 / Other values ​​within the range of N·m.

[0062] The silicon-doped diamond-like composite lubricating coating provided by the present invention can form a complete amorphous carbon transfer film in situ at the friction pair during the friction process.

[0063] As mentioned above, the silicon-doped diamond-like composite lubricating coating provided by the present invention can have better hardness, toughness, wear resistance and crack resistance than traditional DLC coatings. It has lower internal stress and higher toughness, and can effectively resist external wear and impact. Moreover, when the silicon-doped diamond-like composite lubricating coating is rubbed in a high-temperature atmospheric environment, the complete amorphous carbon transfer film formed in situ at the friction pair can effectively reduce the friction coefficient to, so that it has excellent lubrication and friction reduction effect at high temperatures.

[0064] Correspondingly, the present invention also provides a method for preparing the above silicon-doped diamond-like carbon composite lubricating coating, comprising the following steps: sequentially arranging a SiC primer layer and a Si-DLC functional layer on the surface of a substrate.

[0065] In some embodiments, the SiC base layer is prepared by DC magnetron sputtering.

[0066] The preparation conditions of SiC bottom layer may include: the vacuum degree in the equipment chamber is better than 1.0×10 -3 Pa, 50 sccm to 80 sccm (such as 50 sccm, 55 sccm, 60 sccm, 65 sccm, 70 sccm, 75 sccm or 80 sccm, etc.) of argon is introduced into the equipment, and the gas pressure is maintained at 0.2 Pa to 0.3 Pa (such as 0.2 Pa, 0.25 Pa or 0.3 Pa, etc.); the substrate bias voltage is -50 V to -100 V (such as -50 V, -55 V, -6 0V, -65V, -70V, -75V, -80V, -85V, -90V, -95V or -100V, etc.), the bias duty cycle is 50% to 60% (such as 50%, 55% or 60%, etc.), the target current is 1.0A to 2.0A (such as 1.0A, 1.5A or 2.0A, etc.), and the deposition time is 20min to 30min (such as 20min, 25min or 30min, etc.).

[0067] The target material used in the preparation process of the above-mentioned SiC base layer is a graphite-silicon composite target, wherein the Si content can be 35wt% to 45wt%, such as 35wt%, 36wt%, 37wt%, 38wt%, 39wt%, 40wt%, 41wt%, 42wt%, 43wt%, 44wt% or 45wt%, etc., or it can be other values ​​within the range of 35wt% to 45wt%.

[0068] In some embodiments, the Si-DLC functional layer is prepared by using a high-power pulsed magnetron sputtering technology assisted by an anode ion source.

[0069] Preparation conditions of the Si-DLC functional layer may include: an argon gas flow rate of 50 sccm to 80 sccm (such as 50 sccm, 55 sccm, 60 sccm, 65 sccm, 70 sccm, 75 sccm or 80 sccm, etc.), a gas pressure of 0.2 Pa to 0.3 Pa (such as 0.2 Pa, 0.25 Pa or 0.3 Pa, etc.); a substrate bias of -50 V to -100 V (such as -50 V, -55 V, -60 V, -65 V, -70 V, -75 V, -80 V, -85 V, -90 V, -95 V or -100 V, etc.), a bias duty cycle of 50% to 60% (such as 50%, 55% or 60%, etc.); a C-Si composite target is used, and the Si content accounts for 5wt% to 10wt% (such as 5wt%, 6wt%, 7wt%, 8wt%, 9wt%). % or 10wt%), the HiPIMS pulse power is 5.0kW~8.0kW (such as 5.0kW, 5.5kW, 6.0kW, 6.5kW, 7.0kW, 7.5kW or 8.0kW, etc.), the duty cycle is 1.0%~5.0% (such as 1.0%, 1.5%, 2.0%, 2.5%, 3.0%, 3.5%, 4.0%, 4.5% or 5.0%, etc.); the anode layer The anode layer ion source power corresponding to the ion source assisting the ionization of the sputtering gas is 0.50kW~0.75kW (such as 0.50kW, 0.55kW, 0.60kW, 0.65kW, 0.70kW or 0.75kW, etc.), and the duty cycle is 50%~60% (such as 50%, 55% or 60%, etc.); the deposition time is 6h~10h (such as 6h, 7h, 8h, 9h or 10h, etc.).

[0070] Compared with the existing coating equipment in industrial production, the high-power pulsed magnetron sputtering deposition technology assisted by the anode layer ion source has a very high ionization rate, and uses a separate ion source to increase the ionization rate of the sputtering gas. The bombardment energy of the coating system is higher, and it is easier to prepare a composite lubricating coating with special properties under lower temperature conditions (≤100°C). The equipment is simple to operate, which is conducive to mass industrial production.

[0071] For reference, the equipment used in the high-power pulsed magnetron sputtering deposition technology assisted by the anode layer ion source in this application mainly includes a vacuum chamber, a turret system, a high-power pulse power supply, a DC power supply, an anode layer ion source, an air intake unit and a molecular pump, wherein the anode layer ion source, the DC power supply and the high-power pulse power supply are evenly distributed on the inner wall of the vacuum chamber, and a turret capable of revolution and rotation is provided in the vacuum chamber. The high-power pulse power supply and the DC power supply are installed in parallel on the C-Si composite target, and the substrate is installed on the turret. Regarding the equipment and deposition principle used for the high-power pulsed magnetron sputtering and DC magnetron sputtering deposition assisted by the anode layer ion source, reference can be made to the relevant contents of high-power pulsed magnetron sputtering and DC magnetron sputtering, and no excessive restrictions are made here.

[0072] In some embodiments, before preparing the SiC base layer, the method further includes pre-treating the substrate.

[0073] The pretreatment includes grinding and polishing the substrate, then ultrasonic cleaning, and then placing the obtained substrate on a rotating rack in a vacuum chamber and performing plasma glow cleaning using an anode layer ion source.

[0074] Among them, ultrasonic cleaning refers to ultrasonic cleaning in alkaline cleaning agent and deionized water, and the ultrasonic cleaning time can be 40min to 50min, such as 40min, 45min or 50min, etc., and can also be other values ​​within the range of 40min to 50min.

[0075] Plasma glow cleaning may include placing the substrate in a vacuum chamber and evacuating the chamber to a vacuum better than 1.0×10 -3 Pa, then introduce 100 sccm to 150 sccm (such as 100 sccm, 110 sccm, 120 sccm, 130 sccm, 140 sccm or 150 sccm, etc.) of argon gas, and adjust the gas pressure to 0.36 Pa to 0.52 Pa (such as 0.36 Pa, 0.42 Pa, 0.48 Pa or 0.52 Pa, etc.); at the same time, adjust the substrate bias voltage to -1000 V to -1200 V (such as -1000 V, -1050 V, -1100 V, -1150 V or -1200V, etc.), the bias duty cycle is 50% to 60% (such as 50%, 55% or 60%, etc.); then the anode layer ion source is turned on, the anode layer ion source power is 0.8kW to 1.0kW (such as 0.8kW, 0.85kW, 0.9kW, 0.95kW or 1.0kW, etc.), the duty cycle is 50% to 60% (such as 50%, 55% or 60%, etc.), and the plasma glow cleaning time is 30min to 40min (such as 30min, 35min or 40min, etc.).

[0076] As mentioned above, the silicon-doped diamond-like composite lubricating coating provided by the present invention, wherein the silicon element doping significantly changes the microstructure and performance of the DLC coating, can not only reduce its internal stress, but also improve its wear resistance. The coating structure is designed to be a double-layer structure including a base layer of a columnar structure and a functional layer of a dense featureless structure, wherein the base layer presents a tensile stress state, and the functional layer presents a compressive stress state, and when the coating is bent, the stresses of the two will compensate each other, effectively preventing the coating from cracking. In the process of realizing this structural design, DC magnetron sputtering is used to deposit the base layer and an advanced anode layer ion source is used to assist the high-power pulsed magnetron sputtering equipment to deposit the functional layer. High-power pulsed magnetron sputtering technology can generate high-energy plasma, and significantly improve the ionization rate of the sputtering gas through the assistance of the ion source, thereby enhancing the bombardment energy during the deposition process. This series of optimizations not only improves the quality of the film, but also brings significant improvements in its toughness, wear resistance, bonding strength and other key properties. Compared with traditional magnetron sputtering equipment, high-power pulsed magnetron sputtering technology assisted by the anode layer ion source can prepare a composite lubricating coating with special properties at temperatures below 100°C.

[0077] Through the specific preparation method and preparation conditions provided by the present invention, a silicon-doped diamond-like composite lubricating coating having excellent hardness, toughness, wear resistance and crack resistance is effectively prepared.

[0078] In addition, the present invention also provides an application of the silicon-doped diamond-like composite lubricating coating. For example, the silicon-doped diamond-like composite lubricating coating can be used to be disposed on a hard substrate or a flexible substrate in the mechanical, electronic, or medical fields.

[0079] The hard substrate may include stainless steel or hard alloy by way of example but not limitation. The flexible substrate may include polymer, metal foil, thin glass or textile by way of example but not limitation.

[0080] It should be emphasized that by preparing the silicon-doped diamond-like composite lubricating coating provided by the present invention on the surface of a flexible substrate, cracking or breaking of the substrate in a bent state can be effectively avoided.

[0081] The highly tough and wear-resistant silicon-doped diamond-like composite lubricating coating provided by the present invention and its preparation method and application are specifically described below.

[0082] Example 1

[0083] This embodiment provides a high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating, which is prepared by the following method:

[0084] S1: substrate pretreatment.

[0085] The 5 mm thick 304 stainless steel sheet substrate was ultrasonically cleaned with alkaline detergent and deionized water for 45 min, and then the dried substrate was mounted on a rotating rack. The vacuum was then evacuated, and the background vacuum was better than 1.0×10 -3 Pa; introduce 100 sccm argon gas and adjust the gas pressure to 0.36 Pa; adjust the substrate bias to -1100 V and the duty cycle to 55%; turn on the anode layer ion source, set the power to 1.0 kW and the duty cycle to 55%, and perform glow cleaning on the substrate for 40 minutes.

[0086] S2: Preparing a SiC base layer on the surface of the substrate.

[0087] After glow cleaning, adjust the argon flow rate to 70sccm, maintain the gas pressure at 0.26Pa, the substrate bias to -50V, and the duty cycle to 55%; use a C-Si composite target with a Si content of 40wt%; turn on the DC power supply, set the current to 1.0A, and the deposition time to 20min to form a SiC base layer.

[0088] S3: Preparing a Si-DLC functional layer on the surface of the SiC base layer.

[0089] After the SiC base deposition is completed, the argon flow rate is 50sccm, the gas pressure is maintained at 0.20Pa, the substrate bias is -50V, the duty cycle is 55%, the DC power supply is turned off, and the high-power pulsed magnetron sputtering power supply is turned on for deposition. A C-Si composite target is used, the Si content accounts for 6wt%, the HiPIMS pulse power is 7.5kW, and the duty cycle is 1.0%; at the same time, the anode layer ion source is turned on for auxiliary ionization, the anode layer ion source power is 0.60kW, the duty cycle is 55%, and the deposition time is 8h. The rotation speed of the rotating frame is stable at 2rpm during the entire deposition process, and it is naturally cooled after the preparation is completed.

[0090] Figure 1 This is a scanning electron microscope photo of the cross section of the coating sample prepared in this embodiment, which shows, from bottom to top, a 304 stainless steel substrate, a SiC base layer, and a Si-DLC functional layer; it can be observed from this photo that the Si-DLC functional layer can grow well on the SiC base layer. In addition, the Si-DLC functional layer presents a dense featureless structure, and the SiC base layer presents a distinct columnar structure.

[0091] After testing, the total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this embodiment is 2.63μm, of which the thickness of the SiC base layer is 0.37μm and the thickness of the Si-DLC functional layer is 2.26μm. The mass percentage of Si in the SiC base layer is 29.95%, and the mass percentage of C is 70.05%. In the Si-DLC functional layer, the mass percentage of Si is 2.95%, and the mass percentage of DLC is 97.05%.

[0092] Example 2

[0093] The difference between this embodiment and embodiment 1 is that the substrate of this embodiment is a YG6 cemented carbide sheet with a thickness of 5 mm.

[0094] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.66 μm, of which the thickness of the SiC base layer is 0.38 μm and the thickness of the Si-DLC functional layer is 2.28 μm.

[0095] Example 3

[0096] The difference between this embodiment and embodiment 1 is that the substrate of this embodiment is a flexible thin glass with a thickness of 0.1 mm.

[0097] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.50 μm, of which the thickness of the SiC base layer is 0.35 μm and the thickness of the Si-DLC functional layer is 2.15 μm.

[0098] Example 4

[0099] The difference between this embodiment and embodiment 1 is that the substrate of this embodiment is a metal aluminum foil with a thickness of 0.03 mm.

[0100] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.59 μm, of which the thickness of the SiC base layer is 0.34 μm and the thickness of the Si-DLC functional layer is 2.25 μm.

[0101] Example 5

[0102] The difference between this embodiment and embodiment 1 is that in this embodiment, the substrate bias voltage is -80V when depositing the Si-DLC functional layer.

[0103] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.48 μm, of which the thickness of the SiC base layer is 0.36 μm and the thickness of the Si-DLC functional layer is 2.12 μm.

[0104] Example 6

[0105] The difference between this embodiment and embodiment 1 is that in this embodiment, the substrate bias voltage is -100V when depositing the Si-DLC functional layer.

[0106] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.42 μm, of which the thickness of the SiC base layer is 0.34 μm and the thickness of the Si-DLC functional layer is 2.08 μm.

[0107] Example 7

[0108] The difference between this embodiment and embodiment 1 is that in this embodiment, 50 sccm of argon gas is introduced during the deposition of the Si-DLC functional layer, and the gas pressure is adjusted to 0.20 Pa.

[0109] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.34 μm, of which the thickness of the SiC base layer is 0.32 μm and the thickness of the Si-DLC functional layer is 2.02 μm.

[0110] Example 8

[0111] The difference between this embodiment and embodiment 1 is that in this embodiment, 80 sccm of argon gas is introduced when depositing the Si-DLC functional layer, and the gas pressure is adjusted to 0.30 Pa.

[0112] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.91 μm, of which the thickness of the SiC base layer is 0.39 μm and the thickness of the Si-DLC functional layer is 2.52 μm.

[0113] Example 9

[0114] The difference between this embodiment and embodiment 1 is that the deposition time of the Si-DLC functional layer in this embodiment is 6 hours.

[0115] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.38 μm, of which the thickness of the SiC base layer is 0.37 μm and the thickness of the Si-DLC functional layer is 2.01 μm.

[0116] Example 10

[0117] The difference between this embodiment and embodiment 1 is that the deposition time of the Si-DLC functional layer in this embodiment is 10 hours.

[0118] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 4.86 μm, of which the thickness of the SiC base layer is 0.38 μm and the thickness of the Si-DLC functional layer is 4.48 μm.

[0119] Embodiment 11

[0120] The difference between this embodiment and embodiment 1 is that the HiPIMS pulse power during the deposition of the Si-DLC functional layer in this embodiment is 5.0 kW.

[0121] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.41 μm, of which the thickness of the SiC base layer is 0.39 μm and the thickness of the Si-DLC functional layer is 2.02 μm.

[0122] Example 12

[0123] The difference between this embodiment and embodiment 1 is that the HiPIMS pulse power during the deposition of the Si-DLC functional layer in this embodiment is 8.0 kW.

[0124] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 3.06 μm, of which the thickness of the SiC base layer is 0.38 μm and the thickness of the Si-DLC functional layer is 2.68 μm.

[0125] Embodiment 13

[0126] This embodiment is similar to Embodiment 1 except that the power of the anode layer ion source in this embodiment is 0.50 kW.

[0127] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 3.02 μm, of which the thickness of the SiC base layer is 0.40 μm and the thickness of the Si-DLC functional layer is 2.62 μm.

[0128] Embodiment 14

[0129] The difference between this embodiment and embodiment 1 is that the power of the anode layer ion source in this embodiment is 0.75 kW.

[0130] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this embodiment is 2.56 μm, of which the thickness of the SiC base layer is 0.34 μm and the thickness of the Si-DLC functional layer is 2.22 μm.

[0131] Embodiment 15

[0132] This embodiment provides a high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating, which is prepared by the following method:

[0133] S1: substrate pretreatment.

[0134] The 5 mm thick 304 stainless steel sheet substrate was ultrasonically cleaned with alkaline detergent and deionized water for 40 min, and then the dried substrate was mounted on a rotating rack. The vacuum was then evacuated, and the background vacuum was better than 1.0×10 -3 Pa; introduce 120sccm argon gas and adjust the gas pressure to 0.46Pa; adjust the substrate bias to -1000V and the duty cycle to 50%; turn on the anode layer ion source, set the power to 0.8kW and the duty cycle to 50%, and perform glow cleaning on the substrate for 30min.

[0135] S2: Preparing a SiC base layer on the surface of the substrate.

[0136] After glow cleaning, adjust the argon flow rate to 50sccm, maintain the gas pressure at 0.20Pa, the substrate bias to -75V, and the duty cycle to 50%; use a C-Si composite target with a Si content of 35wt%; turn on the DC power supply, set the current to 1.5A, and the deposition time to 25min to form a SiC base layer.

[0137] S3: Preparing a Si-DLC functional layer on the surface of the SiC base layer.

[0138] After the SiC base deposition is completed, the argon flow rate is 65sccm, the gas pressure is maintained at 0.25Pa, the substrate bias is -75V, the duty cycle is 50%, the DC power supply is turned off, and the high-power pulsed magnetron sputtering power supply is turned on for deposition. A C-Si composite target is used, the Si content accounts for 5wt%, the HiPIMS pulse power is 5.0kW, and the duty cycle is 3.0%; at the same time, the anode layer ion source is turned on for auxiliary ionization, the anode layer ion source power is 0.50kW, the duty cycle is 50%, and the deposition time is 6h. The rotation speed of the rotating frame is stable at 2rpm during the entire deposition process, and it is naturally cooled after the preparation is completed.

[0139] The total thickness of the silicon-doped diamond-like composite lubricating coating obtained in this embodiment is 2.35 μm, wherein the thickness of the SiC base layer is 0.31 μm, and the thickness of the Si-DLC functional layer is 2.04 μm. The mass percentage of Si in the SiC base layer is 25.35%, and the mass percentage of C is 75.65%. In the Si-DLC functional layer, the mass percentage of Si is 2.35%, and the mass percentage of DLC is 97.65%.

[0140] Example 16

[0141] This embodiment provides a high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating, which is prepared by the following method:

[0142] S1: substrate pretreatment.

[0143] The 5 mm thick 304 stainless steel sheet substrate was ultrasonically cleaned with alkaline detergent and deionized water for 50 min, and then the dried substrate was mounted on a rotating rack. Then, the vacuum was evacuated, and the background vacuum was better than 1.0×10 -3 Pa; introduce 150sccm argon gas and adjust the gas pressure to 0.52Pa; adjust the substrate bias to -1200V and the duty cycle to 60%; turn on the anode layer ion source, set the power to 1.0kW and the duty cycle to 60%, and perform glow cleaning on the substrate for 35min.

[0144] S2: Preparing a SiC base layer on the surface of the substrate.

[0145] After glow cleaning, adjust the argon flow rate to 80sccm, maintain the gas pressure at 0.30Pa, the substrate bias to -100V, and the duty cycle to 60%; use a C-Si composite target with a Si content of 32wt%; turn on the DC power supply, set the current to 2.0A, and the deposition time to 30min to form a SiC base layer.

[0146] S3: Preparing a Si-DLC functional layer on the surface of the SiC base layer.

[0147] After the SiC base layer deposition is completed, the argon flow rate is 80sccm, the gas pressure is maintained at 0.30Pa, the substrate bias is -100V, the duty cycle is 60%, the DC power supply is turned off, and the high-power pulsed magnetron sputtering power supply is turned on for deposition. A C-Si composite target is used, the Si content accounts for 7wt%, the HiPIMS pulse power is 8.0kW, and the duty cycle is 5.0%; at the same time, the anode layer ion source is turned on for auxiliary ionization, the anode layer ion source power is 0.75kW, the duty cycle is 60%, and the deposition time is 10h. The rotation speed of the rotating frame is stable at 2rpm during the entire deposition process, and it is naturally cooled after the preparation is completed.

[0148] The total thickness of the silicon-doped diamond-like composite lubricating coating obtained in this embodiment is 4.91 μm, wherein the thickness of the SiC base layer is 0.39 μm, and the thickness of the Si-DLC functional layer is 4.52 μm. The mass percentage of Si in the SiC base layer is 31.46%, and the mass percentage of C is 68.54%. In the Si-DLC functional layer, the mass percentage of Si is 3.55%, and the mass percentage of DLC is 96.45%.

[0149] Comparative Example 1

[0150] The difference between this comparative example and Example 1 is that this comparative example deposits the Si-DLC functional layer by DC magnetron sputtering, and the conditions of DC magnetron sputtering include: the argon flow rate is 50sccm, the gas pressure is maintained at 0.20Pa, the substrate bias is -50V, the duty cycle is 55%, the DC power supply is turned on for deposition, a C-Si composite target is used, the Si content accounts for 6wt%, the DC target current is 1.5A, and the DC target voltage is 500V; at the same time, the anode layer ion source is turned on for auxiliary ionization, the anode layer ion source power is 0.60kW, the duty cycle is 55%, and the deposition time is 8h. The rotation speed of the rotating frame is stabilized at 2rpm during the entire deposition process, and it is naturally cooled after the preparation is completed.

[0151] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this comparative example is 2.94 μm, of which the thickness of the SiC base layer is 0.38 μm and the thickness of the Si-DLC functional layer is 2.56 μm.

[0152] Comparative Example 2

[0153] The difference between this comparative example and Example 1 is that the Ar flow rate during the preparation of the Si-DLC functional layer is 150 sccm and the gas pressure is maintained at 0.6 Pa.

[0154] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.82 μm, of which the thickness of the SiC base layer is 0.43 μm and the thickness of the Si-DLC functional layer is 2.39 μm.

[0155] Comparative Example 3

[0156] The difference between this comparative example and Example 1 is that the substrate bias voltage during the preparation of the Si-DLC functional layer is 0V.

[0157] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.72 μm, of which the thickness of the SiC base layer is 0.46 μm and the thickness of the Si-DLC functional layer is 2.26 μm.

[0158] Comparative Example 4

[0159] The difference between this comparative example and Example 1 is that the ion source power of the anode layer during the preparation of the Si-DLC functional layer is 0 W.

[0160] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.65 μm, of which the thickness of the SiC base layer is 0.39 μm and the thickness of the Si-DLC functional layer is 2.26 μm.

[0161] Comparative Example 5

[0162] The difference between this comparative example and Example 1 is that the power of the anode layer ion source during the preparation of the Si-DLC functional layer is 1.0 kW.

[0163] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating of this comparative example is 1.92 μm, of which the thickness of the SiC base layer is 0.34 μm and the thickness of the Si-DLC functional layer is 1.58 μm.

[0164] Comparative Example 6

[0165] The difference between this comparative example and Example 1 is that in this comparative example, no SiC base layer is deposited.

[0166] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating obtained in this comparative example is 2.26 μm, wherein the thickness of the SiC primer layer is 0 μm, and the thickness of the Si-DLC functional layer is 2.26 μm.

[0167] Comparative Example 7

[0168] The difference between this comparative example and Example 1 is that the substrate of this comparative example is carbon steel.

[0169] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like carbon composite lubricating coating of this comparative example is 2.63 μm, of which the thickness of the SiC primer layer is 0.37 μm and the thickness of the Si-DLC functional layer is 2.26 μm.

[0170] Comparative Example 8

[0171] The difference between this comparative example and Example 1 is that an undoped DLC coating is prepared in this comparative example.

[0172] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.63 μm, of which the thickness of the SiC base layer is 0.37 μm and the thickness of the Si-DLC functional layer is 2.26 μm.

[0173] Comparative Example 9

[0174] The difference between this comparative example and Example 1 is that the tungsten-doped diamond-like carbon coating in this comparative example is prepared by the same process.

[0175] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.72 μm, of which the thickness of the SiC base layer is 0.37 μm and the thickness of the W-DLC functional layer is 2.35 μm.

[0176] Comparative Example 10

[0177] The difference between this comparative example and Example 1 is that the boron-doped diamond-like coating in this comparative example is prepared by the same process.

[0178] The total thickness of the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in this comparative example is 2.63 μm, of which the thickness of the SiC base layer is 0.37 μm and the thickness of the B-DLC functional layer is 2.26 μm.

[0179] Comparative Example 11

[0180] The difference between this comparative example and Example 1 is that the preparation parameter range of the SiC base layer is adjusted so that the thickness of the SiC base layer is 0.18 μm.

[0181] Comparative Example 12

[0182] The difference between this comparative example and Example 1 is that the preparation parameter range of the SiC base layer is adjusted so that the thickness of the SiC base layer is 0.50 μm.

[0183] Comparative Example 13

[0184] The difference between this comparative example and Example 1 is that the preparation parameter range of the Si-DLC functional layer is adjusted so that the thickness of the Si-DLC functional layer is 1.20 μm.

[0185] Comparative Example 12

[0186] The difference between this comparative example and Example 1 is that the preparation parameter range of the Si-DLC functional layer is adjusted so that the thickness of the Si-DLC functional layer is 6.0 μm.

[0187] Comparative Example 13

[0188] The difference between this comparative example and Example 1 is that the preparation parameter range of the SiC base layer is adjusted so that the mass percentage of Si in the SiC base layer is 20.05% and the mass percentage of C is 79.95%.

[0189] Comparative Example 14

[0190] The difference between this comparative example and Example 1 is that the preparation parameter range of the SiC base layer is adjusted so that the mass percentage of Si in the SiC base layer is 50.25% and the mass percentage of C is 49.75%.

[0191] Comparative Example 15

[0192] The difference between this comparative example and Example 1 is that the preparation parameter range of the Si-DLC functional layer is adjusted so that the mass percentage of Si in the Si-DLC functional layer is 1.20% and the mass percentage of DLC is 98.8%.

[0193] Comparative Example 16

[0194] The difference between this comparative example and Example 1 is that the preparation parameter range of the Si-DLC functional layer is adjusted so that the mass percentage of Si in the Si-DLC functional layer is 14.0% and the mass percentage of DLC is 86.0%.

[0195] Test example

[0196] ①. The silicon-doped diamond-like composite lubricating coatings prepared in Examples 2 to 16 were subjected to structural tests. The results showed that the Si-DLC functional layers of the silicon-doped diamond-like composite lubricating coatings prepared in the above examples all had a dense featureless structure, and the SiC base layers all had an obvious columnar structure.

[0197] ②, A, the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1 was partially tested for performance, and the results are shown in Table 1 and Figure 2 shown. Figure 2 This is a load-displacement curve of the high-strength, toughness, and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in Example 1, wherein Ee is the area between the loading curve and the unloading curve, representing the energy dissipated in the coating due to plastic deformation; Ep is the area under the unloading curve, representing the elastic energy of the deformation.

[0198] The hardness in Table 1 is measured with reference to GB / T 33051-2016 Determination of the thickness of the hardened layer of optical functional film surface hardening film; the equivalent elastic modulus E* is calculated according to the following formula: E* = E / (1-ν 2 ), where E refers to elastic modulus and ν refers to Poisson's ratio; the hardness modulus ratio data is rounded off; the elastic recovery coefficient is measured with reference to GB / T 43602-2023 Composition, structure and performance evaluation of physical vapor deposition multilayer hard coatings; the internal stress is measured with reference to the laser curvature method and Stony formula calculation method.

[0199] In addition, the same performance tests were performed on the coatings obtained in Examples 2 to 16 and Comparative Examples 1 to 16, and the results are also shown in Table 1.

[0200] B. The high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating obtained in Example 1 was subjected to bending tests at different angles at 30°, 60°, 90° and 120°. The photos after the test and the optical morphology photos of the corresponding folds are shown in FIG. Figure 3 shown.

[0201] It can be seen from the figure that the silicon-doped diamond-like composite lubricating coating prepared on the 304 stainless steel substrate provided in Example 1 did not crack or peel off after bending and flattening tests at different angles of 0° (corresponding to column a), 30° (corresponding to column b), 60° (corresponding to column c), 90° (corresponding to column d), and 120° (corresponding to column e), and the coating has very excellent anti-cracking performance.

[0202] It should be noted that, taking column a as an example, a1 is the result of the physical object at the first viewing angle, a2 is the result of the physical object at the second viewing angle, and a3 is the optical morphology result of the surface of the physical object at the corresponding fold.

[0203] In the same manner, the silicon-doped diamond-like composite lubricating coatings prepared in Examples 2 to 16 did not crack or peel off after being bent and flattened at different angles of 30°, 60°, 90°, and 120°.

[0204] In the same manner, the silicon-doped diamond-like composite lubricating coatings prepared in Comparative Examples 1 to 16 also cracked and peeled off after bending and flattening tests at different angles of 30°, 60°, 90°, and 120°.

[0205] C. The high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating prepared in Example 1 is mixed with Al 2 O 3 The friction pair was subjected to friction tests at a room temperature of 25°C and a high temperature of 450°C. The friction time of the friction test at 25°C was 3600s, and the friction time of the friction test at 450°C was 900s. The results are shown in Figure 4 (a) and (b) and Table 2. In addition, the above experiment also shows that the wear debris generated at the wear scar after high temperature friction is transferred to the surface of the grinding ball to form a complete friction transfer film, resulting in its excellent lubrication and friction reduction effect.

[0206] Furthermore, the same performance tests were performed on the coatings obtained in Examples 2 to 16 and Comparative Examples 1 to 16, and the results are also shown in Table 2.

[0207] Table 1 Performance results

[0208]

[0209]

[0210] Table 2 Performance results

[0211]

[0212]

[0213] It can be seen from this that the high-toughness and wear-resistant silicon-doped diamond-like composite lubricating coating provided by the embodiment of the present invention has excellent anti-cracking performance and a low friction coefficient in a high-temperature atmospheric environment.

[0214] In summary, the solution provided by the present invention has at least the following advantages:

[0215] (1) The high-strength, tough and wear-resistant silicon-doped diamond-like composite lubricating coating provided by the present invention can simultaneously have high hardness, toughness, wear resistance and crack resistance, and the silicon-doped diamond-like composite lubricating coating has a dense structure. Compared with traditional DLC coatings, the silicon-doped diamond-like composite lubricating coating provided by the present invention has lower internal stress and higher toughness, and can effectively resist external wear and impact.

[0216] (2) The highly tough and wear-resistant silicon-doped diamond-like composite lubricating coating provided by the present invention can form a complete amorphous carbon transfer film in situ at the friction pair during friction, effectively reducing the friction coefficient and having excellent lubrication and friction reduction effects even at high temperatures.

[0217] (3) The high-strength, tough and wear-resistant silicon-doped diamond-like composite lubricating coating provided by the present invention is prepared by using an ion source-assisted high-power pulsed magnetron sputtering coating system. Compared with the conventional magnetron sputtering equipment in existing industrial production, the use of an ion source-assisted high-power pulsed magnetron sputtering coating system for preparation increases the bombardment energy during the thin film deposition process, making it easier to prepare a hard nano-composite lubricating coating with special properties.

[0218] (4) The present invention provides a preparation method using ion source-assisted high-power pulsed magnetron sputtering technology. The coating deposited in a low-temperature environment (≤100°C) makes it suitable for flexible substrates such as polymer foils, thin glass, and textiles. It can also be applied to flexible electronic devices, flat panel displays, and flexible moving parts such as micro-electromechanical devices in high-temperature environments, thereby broadening its application range.

[0219] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A silicon-doped diamond-like composite lubricating coating, characterized in that: The silicon-doped diamond-like composite lubricating coating comprises a SiC primer layer and a Si-DLC functional layer which are sequentially arranged on the surface of a substrate; The SiC base layer has a columnar structure, and the thickness of the SiC base layer is 0.3 μm to 0.4 μm; the Si-DLC functional layer has a dense featureless structure, and the thickness of the Si-DLC functional layer is 2.0 μm to 5.0 μm.

2. The silicon-doped diamond-like composite lubricating coating according to claim 1, characterized in that: In the SiC base layer, the mass percentage of Si is 25% to 35%, and the mass percentage of C is 65% to 75%.

3. The silicon-doped diamond-like composite lubricating coating according to claim 1, characterized in that: In the Si-DLC functional layer, the mass percentage of Si is 2% to 8%, and the mass percentage of DLC is 92% to 98%.

4. The silicon-doped diamond-like composite lubricating coating according to any one of claims 1 to 3, characterized in that: The silicon-doped diamond-like composite lubricating coating has at least one of the following characteristics: Feature 1: The hardness of the silicon-doped diamond-like composite lubricating coating is H, and the range of H is 18GPa to 25GPa; preferably, H is 18.0GPa to 24.6GPa; Feature 2: The equivalent elastic modulus of the silicon-doped diamond-like composite lubricating coating is E*, H / E*≥0.1; preferably, H / E* is 0.102-0.106; Feature 3: The elastic recovery coefficient of the silicon-doped diamond-like composite lubricating coating is We, We ≥ 60%; preferably, We is 76.5% to 82.2%; Feature 4: The silicon-doped diamond-like composite lubricating coating is in a compressive stress state as a whole; preferably, the SiC base layer is in a tensile stress state, and the Si-DLC functional layer is in a compressive stress state; Feature 5: The microstructure of the silicon-doped diamond-like composite lubricating coating is dense; Feature 6: The friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 25°C is 0.07 to 0.08; preferably, the friction coefficient is 0.072 to 0.079; Feature 7: The friction coefficient of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450° C. is 0.040 to 0.065; preferably, the friction coefficient is 0.040 to 0.063; Feature 8: The wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment of 25°C is no more than 10 -7 m 3 / N·m; Feature 9: The wear rate of the silicon-doped diamond-like composite lubricating coating in an atmospheric environment at 450°C is no more than 10 -6 m 3 / N·m; Feature 10: During the friction process, the silicon-doped diamond-like composite lubricating coating forms a complete amorphous carbon transfer film in situ at the friction pair.

5. A method for preparing a silicon-doped diamond-like composite lubricating coating according to any one of claims 1 to 4, characterized in that: The following steps are involved: The SiC base layer and the Si-DLC functional layer are sequentially arranged on the surface of the substrate.

6. The preparation method according to claim 5, characterized in that: The SiC base layer is prepared by a DC magnetron sputtering method; The preparation conditions of the SiC bottom layer include: the vacuum degree in the equipment chamber is better than 1.0×10 -3 Pa, 50sccm~80sccm argon gas is introduced into the equipment, and the gas pressure is maintained at 0.2Pa~0.3Pa; the substrate bias is -50V~-100V, and the bias duty cycle is 50%~60%; the target current is 1.0A~2.0A, and the deposition time is 20min~30min; Preferably, the target material is a graphite-silicon composite target, wherein the Si content accounts for 35wt% to 45wt%.

7. The preparation method according to claim 5, characterized in that: The Si-DLC functional layer is prepared by high-power pulsed magnetron sputtering technology assisted by an anode ion source; The preparation conditions of the Si-DLC functional layer include: an argon gas flow rate of 50 sccm to 80 sccm and a gas pressure of 0.2 Pa to 0.3 Pa; a substrate bias of -50 V to -100 V and a bias duty cycle of 50% to 60%; a C-Si composite target with a Si content of 5 wt% to 10 wt%, a HiPIMS pulse power of 5.0 kW to 8.0 kW and a duty cycle of 1.0% to 5.0%; an anode layer ion source power of 0.50 kW to 0.75 kW corresponding to auxiliary ionization of the sputtering gas and a duty cycle of 50% to 60%; and a deposition time of 6 h to 10 h.

8. The preparation method according to any one of claims 5 to 7, characterized in that: Before preparing the SiC base layer, the method further includes pre-treating the substrate; Preferably, the pretreatment includes grinding and polishing the substrate, then ultrasonic cleaning, and then placing the obtained substrate on a rotating rack in a vacuum chamber and performing plasma glow cleaning using an anode layer ion source.

9. The preparation method according to claim 8, characterized in that: Ultrasonic cleaning time is 40min to 50min; And / or, the plasma glow cleaning comprises: placing the substrate in a vacuum chamber, evacuating the vacuum to a value better than 1.0×10 -3 Pa, then introduce 100sccm~150sccm argon gas, and adjust the gas pressure to 0.36Pa~0.52Pa; at the same time, adjust the substrate bias to -1000V~-1200V, and the bias duty cycle is 50%~60%; then turn on the anode layer ion source, the anode layer ion source power is 0.8kW~1.0kW, the duty cycle is 50%~60%, and the plasma glow cleaning time is 30min~40min.

10. An application of the silicon-doped diamond-like composite lubricating coating according to any one of claims 1 to 4, characterized in that: The silicon-doped diamond-like composite lubricating coating is used to be arranged on a hard substrate or a flexible substrate in the fields of mechanics, electronics, or medicine; Preferably, the hard substrate comprises stainless steel or hard alloy; Preferably, the flexible substrate comprises a polymer, a metal foil, a flexible thin glass or a textile.

Citation Information

Patent Citations

  • Hydrogen-free diamond-like carbon film as well as preparation method and application thereof

    CN109136843A

  • Preparation method of Si-doped diamondlike coating layer

    CN109182997A

  • A diamond- and / or diamond-like carbon-coated hard material

    EP0503822A2

  • Covering member having excellent wear resistance and sliding characteristic and method of manufacturing the same

    JP2012121114A

  • Highly wear-resistant thermal print heads with silicon-doped diamond-like carbon protective coatings

    US6046758A