Gold surface modifier, gold surface modification method and surface modified gold
Through the reaction of chloroalic acid and thiol of the gold surface modifier, a gradient structure of gold-thiol-adhesive is formed, which solves the problem of insufficient bonding strength on the gold surface and achieves high-efficiency bonding strength under normal temperature and pressure Improved, suitable for extreme environmental applications of gold printed circuit boards.
Patent Information
- Application Number
- CN202311091590.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-08-28
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to improve the bonding strength between gold and adhesive without damaging the gold surface, and often requires large equipment and complex processes, making it difficult to be suitable for surface treatment of gold printed circuit boards.
A gold surface modifier is used to form a gold-thiol-adhesive gradient structure through the rapid chemical reaction of chloroauric acid and thiol, and introduce the active group thiol group to significantly enhance the bond strength between the gold surface and other materials. And it is processed at room temperature and pressure.
It has achieved significant improvement in the bonding strength between gold and adhesives without damaging the surface of the gold. It is suitable for extreme environments, with simple process and loose conditions, and is suitable for large-scale industrial applications.
Smart Images

Figure CN118979246A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of metal material surface treatment, and more particularly to a gold surface modifier, a gold surface modification method and surface modified gold. Background Art
[0002] Gold atoms are deposited on other metal substrates by chemical deposition and other methods to form a thin layer of gold atoms, which gives the material different properties and can be used in the fields of fine electronics, aerospace and communications, and has a wide range of applications. However, gold atoms are very stable, have low roughness, and have difficult bonding properties, so they are difficult to use. Surface treatment is required to improve the surface bonding strength and enhance its bonding strength in extreme environments such as high temperature or low temperature in order to truly obtain valuable use. There are two existing ways to enhance the surface bonding strength of materials. One is to make the surface of the material uneven by mechanical treatment, such as sandblasting, chemical corrosion, etc., to increase the roughness of the surface of the material. The other is to modify the surface of the material, on the one hand to form a polymer layer, and to improve the bonding strength by improving wettability, etc., and on the other hand to give its surface sufficient bonding activity by introducing active groups, so that the surface can react with various adhesives to form a chemical bond of chemical bonds and improve the bonding strength. Since the atomic layer obtained by chemical deposition is a few microns or even a few nanometers, sandblasting and other treatment methods will destroy the surface gold deposition layer and affect the performance.
[0003] Gold printed circuit boards are currently widely used in modern aviation, aerospace, transportation and other fields. However, due to the high surface inertness of gold, it is difficult for the printed surface to directly produce a strong bonding effect with common adhesives (such as epoxy resins, cyanate resins, etc.), and it needs to be surface treated. The more mature surface treatment methods currently include: mechanical surface treatment, chemical surface etching treatment, and modern surface treatment. Mechanical surface treatment includes sandblasting, shot blasting, grinding, rolling, polishing, brushing, spraying, painting, oiling, etc. The main principle is to remove the loose oxide layer and contamination layer on the surface through treatment, eliminate the weak boundary layer on the surface, increase the surface roughness, increase the effective bonding area and increase the mechanical bonding force, and improve the bonding strength. However, this technology will cause serious damage to the gold surface morphology, and it is difficult to apply it in the current increasingly developed surface bonding enhancement treatment of gold circuit boards. Chemical surface etching treatment includes bluing and blackening, phosphating, pickling, chemical plating of various metals and alloys, TD treatment, QPQ treatment, chemical oxidation, etc. It mainly removes loose metal hydroxides, oxides, etc. on the surface through acid etching and oxidation methods to form a relatively stable oxide layer and metal salt, protect the metal surface from oxidation during use, prevent the desorption of the surface oxide layer, and also increase the surface roughness. However, this technology will cause irreversible etching damage to the surface morphology of gold, and it is difficult to apply it to the treatment of precision printed circuits. Modern surface treatment includes chemical vapor deposition CVD, physical vapor deposition PVD, ion implantation, ion plating, laser surface treatment, etc. This method has strong applicability, but it requires special equipment, the conditions are relatively harsh, the process is complex, it is difficult to promote and use on a large scale, and the treatment efficiency is extremely low. It is currently only used in semiconductor doping, jewelry making and surface treatment scenarios of special materials. The main purpose of this treatment method is to form a surface layer on the metal surface with mechanical, physical and chemical properties different from those of the metal substrate to achieve good bonding properties. These methods are relatively mature and applied to relatively active metal surfaces such as iron, aluminum, steel, and zinc, because the surfaces of these metals are easily oxidized and corroded, causing stress corrosion and desorption at the interface. Therefore, chemical reactions can be used to form a hard and stable porous structure on the surface, and the interfacial bonding strength can be increased through mechanical and adsorption, such as phosphoric acid anodizing of commonly used aluminum alloys, blueing treatment of iron, surface zinc plating and gold plating, and acid etching of stainless steel. However, these methods are extremely ineffective for precious metals with stable chemical properties, such as copper, gold, silver, titanium, and other metals.
[0004] Although most mechanical and chemical treatment methods can increase the bonding strength between gold and adhesives, they inevitably cause irreversible damage to the gold surface, such as destroying the connection of printed circuits and causing circuit failure. Although chemical vapor deposition CVD, physical vapor deposition PVD, ion implantation and other technologies can preserve the surface structure of printed circuits and increase the bonding strength, they rely on a large number of large equipment and have complex operating processes, which seriously affect the processing efficiency. Laser treatment of metal surfaces is a new method at present. Its principle is to rely on the instantaneous high temperature of the laser to form a regular concave and convex structure on the surface. It has been reported on difficult-to-bond metals such as titanium alloys. This technology has high precision and can theoretically ensure the normal operation of printed circuits. However, it still faces the limitations of high equipment requirements, complex processes and high costs. At the same time, the instantaneous temperature of laser treatment can reach more than 1000℃, which will cause serious damage to the substrate of the printed circuit (such as PI, PET and other plastics), making it difficult to apply to the surface treatment of gold printed circuits. Finally, even if laser treatment can form micropores on the gold surface, it is difficult to form wettability with adhesives. This is because, according to wetting theory, when the contact angle is greater than 90°, the rougher the surface, the larger the contact angle, and the more difficult it is to wet.
[0005] In view of this, the development of a new gold surface modifier that can increase the bonding strength between gold and adhesive without causing irreversible damage to the gold surface, without relying on a large number of large equipment and with a simple operation process has become an urgent problem to be solved in this field. Summary of the invention
[0006] In order to solve the problems in the prior art, the present invention provides a gold surface modifier, which reacts rapidly after being coated on the gold surface, and then forms a gold-thiol-adhesive gradient structure after being coated with an adhesive, thereby enhancing the affinity between the gold surface and the adhesive; at the same time, an active group thiol is introduced into the gold surface, so that the gold surface can react to form a covalent bond, significantly improving the bonding strength between the gold surface and other materials, and meeting the bonding requirements in extreme environments. The use conditions of the gold surface modifier are normal temperature and pressure, and the gold surface is treated by a rapid chemical reaction, which neither causes irreversible damage to the gold surface nor relies on a large number of large equipment. The process is simple, the conditions are loose, the raw materials are easily available, and the reaction is rapid, and it has a high engineering application value.
[0007] One of the objects of the present invention is to provide a gold surface modifier, the gold surface modifier comprising a chloroauric acid solution dissolved in a first solvent and a thiol solution dissolved in a second solvent. Preferably, the thiol is a multi-arm thiol; the first solvent is anhydrous ethanol; and the second solvent is acetone. More preferably, the multi-arm thiol is a two-arm thiol, and the two-arm thiol is any one of 1,6-hexanedithiol, 1,5-pentanedithiol, 1,8-octanedithiol, and 1,2-benzenedithiol. Technicians can select appropriate thiol, the first solvent, and the second solvent according to actual needs.
[0008] In one preferred embodiment of the present invention, the concentration of the thiol solution is 10-50wt%, preferably 15-30wt%. The technician can select the appropriate concentration of the thiol solution according to actual needs. The concentration of the chloroauric acid solution is 0.5-2wt%, preferably 1-1.5wt%. The technician can select the appropriate concentration of the chloroauric acid solution according to actual needs.
[0009] In another preferred embodiment of the present invention, the gold surface is a gold printed circuit surface.
[0010] The second object of the present invention is to provide a method for surface modification of gold, which includes two methods. The first method is: applying the chloroauric acid solution described in one of the objects of the present invention to the gold surface, reacting to obtain a first surface-modified gold; applying the thiol solution described in one of the objects of the present invention to the first surface-modified gold, reacting to obtain a surface-modified gold. The second method is: applying the thiol solution described in one of the objects of the present invention to the gold surface, reacting to obtain a first surface-modified gold; applying the chloroauric acid solution described in one of the objects of the present invention to the first surface-modified gold, reacting to obtain a surface-modified gold.
[0011] The first method can be specifically implemented as follows:
[0012] Step 1: Cleaning. The gold to be surface-modified is cleaned by first cleaning its surface with acetone solution to remove grease, dust and other debris. Then, ultrasonically treat it with anhydrous ethanol for 3 minutes, and then ultrasonically treat it with clean water for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set to 80°C to dry the surface moisture.
[0013] Step 2: Prepare a gold surface modifier. A certain concentration of thiol solution is prepared with acetone as solvent, and a certain concentration of chloroauric acid solution is prepared with anhydrous ethanol as solvent, and the two are used together as gold surface modifiers.
[0014] Step 3: Surface treatment. First, use a cotton swab to apply a layer of chloroauric acid solution on the cleaned gold surface so that the parts of the gold surface that need to be coated with adhesive are completely covered. React at room temperature for a period of time until the solvent evaporates and the gold surface is dry to obtain the first surface-modified gold. Secondly, use a cotton swab to apply a layer of thiol solution on the part where the chloroauric acid solution is applied to the first surface-modified gold so that the part is completely covered. React at room temperature for a period of time until the solvent evaporates and the gold surface is dry to obtain the surface-modified gold.
[0015] Step 4, assembly and curing. The surface modified gold is bonded, assembled and cured with other materials through adhesives. After the assembly is completed, the surface modified gold-adhesive-other materials are placed in a blast drying oven for curing. Preferably, the adhesive can be selected from commonly used adhesives such as cyanate adhesives and epoxy resins. Other materials can be aluminum plates, honeycombs and other materials. More preferably, the curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0016] The scheme of the second method is basically the same as the first method, with the only difference being that in step three, first, a layer of thiol solution is applied to the cleaned gold surface with a cotton swab so that the parts of the gold surface that need to be coated with adhesive are completely covered. The reaction is allowed to proceed for a period of time until the solvent evaporates and the gold surface is dry, thereby obtaining the first surface-modified gold. Secondly, a layer of gold chlorate solution is applied to the part of the first surface-modified gold where the thiol solution is applied with a cotton swab so that the part is completely covered. The reaction is allowed to proceed for a period of time until the solvent evaporates and the gold surface is dry, thereby obtaining the surface-modified gold.
[0017] After the gold surface is treated using the above two methods, chloroauric acid and thiol undergo a rapid redox reaction on the gold surface. After coating with adhesive, a gold-thiol-adhesive gradient structure is formed, which greatly increases the affinity between gold and common adhesives. At the same time, the active group thiol is introduced into the gold surface, so that the gold surface can react to form covalent bonds, significantly improving the bonding strength between the gold surface and other materials.
[0018] In one preferred embodiment of the present invention, the reaction time is 5 to 10 minutes. Specifically, in the first method, a layer of chloroauric acid solution is applied on the cleaned gold surface with a cotton swab to obtain the first surface-modified gold by reaction, and the reaction time is 5 to 10 minutes; at the same time, a layer of thiol solution is applied on the first surface-modified gold surface with a cotton swab, and the reaction is allowed to proceed for a period of time, and the reaction time is also 5 to 10 minutes. In the second method, a layer of thiol solution is applied on the cleaned gold surface with a cotton swab to obtain the first surface-modified gold by reaction, and the reaction time is 5 to 10 minutes; at the same time, a layer of chloroauric acid solution is applied on the first surface-modified gold surface with a cotton swab to proceed for a period of time, and the reaction time is also 5 to 10 minutes. Technicians can select the appropriate reaction time according to actual needs.
[0019] The third object of the present invention is to provide a surface modified gold obtained by the surface modification method described in the second object of the present invention.
[0020] Compared with the prior art, the present invention has the following beneficial effects:
[0021] After the gold surface modifier of the present invention is used to treat the gold surface, and then the adhesive is coated to form a gold-thiol-adhesive gradient structure, which enhances the affinity between the gold surface and the adhesive; at the same time, the active group thiol is introduced into the gold surface, so that the gold surface can react to form a covalent bond, which significantly improves the bonding strength between the gold surface and other materials. The gold surface modifier of the present invention can increase the bonding strength between gold and the adhesive through a simple chemical reaction at room temperature and pressure. At the same time, the use of the gold surface modifier will neither cause irreversible damage to the gold surface nor rely on a large number of large equipment. The process is simple, the conditions are loose, the raw materials are easy to obtain, and the reaction is rapid. It can be used on a large scale industrially and is widely used in the technical fields of electronics, aerospace, etc. In addition, the surface-modified gold obtained by the gold surface modifier of the present invention can meet the bonding requirements under extreme environments. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 The preparation method of the surface modified gold printed circuit board-cyanate adhesive film-aluminum plate of the present application;
[0023] Figure 2 This is a scanning electron microscope image of the surface modified gold printed circuit board prepared in Example 1 of the present invention. DETAILED DESCRIPTION
[0024] The present invention is described in detail below in conjunction with specific drawings and embodiments. It is necessary to point out that the following embodiments are only used to further illustrate the present invention and cannot be understood as limiting the scope of protection of the present invention. Some non-essential improvements and adjustments made to the present invention by those skilled in the art based on the content of the present invention still fall within the scope of protection of the present invention.
[0025] In the present invention, the CAS number of tetrachloroauric acid trihydrate (HAuCl4·3H2O) is 16961-25-4, and 1,6-hexanedithiol (C6H 14 S2) with CAS number 1191-43-1, were purchased from Aladdin Biochemical Technology Co., Ltd.
[0026] Example 1
[0027] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0028] (2) Preparation of gold surface modifier: A 1 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 10 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0029] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 10wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 1wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0030] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0031] Example 2
[0032] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0033] (2) Preparation of gold surface modifier: A 1 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 15 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0034] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 15wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 1wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0035] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0036] Example 3
[0037] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0038] (2) Preparation of gold surface modifier: A 1 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 20 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0039] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 20wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 1wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0040] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0041] Example 4
[0042] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0043] (2) Preparation of gold surface modifier: A 1 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 30 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0044] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 30wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 1wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0045] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0046] Example 5
[0047] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0048] (2) Preparation of gold surface modifier: A 1 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 50 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0049] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 50wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 1wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0050] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0051] Example 6
[0052] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0053] (2) Preparation of gold surface modifier: A 0.5 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 15 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0054] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 0.5wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 15wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with 0.5wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0055] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0056] Example 7
[0057] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0058] (2) Preparation of gold surface modifier: A 2 wt% chloroauric acid solution was prepared with anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O); a 15 wt% 1,6-hexanedithiol solution was prepared with acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2). Both chloroauric acid solution and thiol solution are used as gold surface modifiers.
[0059] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 2wt% chloroauric acid solution to the gold printed circuit board, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Apply 15wt% 1,6-hexanedithiol solution to the surface of the gold printed circuit board coated with the 2wt% chloroauric acid solution, and the coating treatment surface is 12.5×25mm. Leave it at room temperature for 10 minutes, wait for the solvent to evaporate until the surface is dry, and obtain a surface-modified gold printed circuit board.
[0060] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0061] Comparative Example 1
[0062] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0063] (2) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the gold printed circuit board of step (1), with a bonding surface of 12.5×25 mm. Cover the 100×25 mm aluminum plate on the position of the cyanate film, with a contact surface of 12.5×25 mm, and assemble the gold printed circuit board-cyanate film-aluminum plate. Put the gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0064] Comparative Example 2
[0065] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0066] (2) Preparation of gold surface modifier: A chloroauric acid solution with a concentration of 1 wt% was prepared using anhydrous ethanol as solvent, and the solute was tetrachloroauric acid trihydrate (HAuCl4·3H2O).
[0067] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 1wt% chloroauric acid solution to the gold printed circuit board, and the applied surface is 12.5×25 mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Obtain a surface-modified gold printed circuit board.
[0068] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0069] Comparative Example 3
[0070] (1) Cleaning: Cut the gold printed circuit board to be surface modified into a size of 100×25 mm, first clean its surface with acetone solution to remove grease, dust and other debris. Then use anhydrous ethanol for ultrasonic treatment for 3 minutes, and then use clean water for ultrasonic treatment for 3 minutes to further clean the residual ethanol. Finally, use a blast drying oven set at 80°C to dry the surface moisture.
[0071] (2) Preparation of gold surface modifier: A 15 wt% 1,6-hexanedithiol solution was prepared using acetone as solvent, and the solute was 1,6-hexanedithiol (C6H 14 S2).
[0072] (3) Surface treatment: After cleaning the surface of the gold printed circuit board, apply the 15 wt% 1,6-hexanedithiol solution to the gold printed circuit board, and the applied surface is 12.5×25 mm. Leave it at room temperature for 10 minutes. Wait for the solvent to evaporate until the surface is dry. Obtain a surface-modified gold printed circuit board.
[0073] (4) Assembly and curing: Paste the cut 12.5×25 mm cyanate film on the surface modified gold printed circuit board in step (3), with a bonding surface of 12.5×25 mm. Cover the cyanate film with a 100×25 mm aluminum plate, with a contact surface of 12.5×25 mm, to obtain a surface modified gold printed circuit board-cyanate film-aluminum plate. Put the surface modified gold printed circuit board-cyanate film-aluminum plate into a forced air drying oven and cure it. The curing process is: first treat at 155°C for 4 hours and then treat at 180°C for 2 hours.
[0074] Figure 1 The invention shows a method for preparing a surface-modified gold printed circuit board-cyanate adhesive film-aluminum plate. Figure 2 The scanning electron microscope image of the surface modified gold printed circuit board prepared in Example 1 is shown. Figure 2 It can be seen that after surface modification, the surface modifier reacted with the surface of the gold printed circuit board, and the thorn-like products played a decisive role in enhancing the bonding strength.
[0075] The surface modified gold printed circuit board-cyanate adhesive film-aluminum plate obtained in Examples 1 to 7 and the gold printed circuit board-cyanate adhesive film-aluminum plate obtained in Comparative Examples 1 to 3 were respectively tested for bonding performance at room temperature and high temperature. The bonding performance test method was based on the tensile shear test standard GB / T 7124-2008. The test results are shown in Tables 1 to 10.
[0076] Table 1 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 1
[0077]
[0078] Table 2 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 2
[0079]
[0080] Table 3 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 3
[0081]
[0082] Table 4 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 4
[0083]
[0084] Table 5 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 5
[0085]
[0086] Table 6 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 6
[0087]
[0088] Table 7 Shear strength of surface modified gold printed circuit board and aluminum plate at room temperature and high temperature in Example 7
[0089]
[0090] Table 8 Tensile shear strength of gold printed circuit board and aluminum plate in comparative example 1 at room temperature and high temperature
[0091] Blank control Room temperature (MPa) High temperature (MPa) (150℃) 1 1.34 0.72 2 1.27 1.12 3 1.09 0.83 4 0.89 0.79 5 0.99 0.58 6 0.85 1.29 average value 1.07 0.89
[0092] Table 9 Tensile shear strength of gold printed circuit board and aluminum plate in comparative example 2 at room temperature and high temperature
[0093] 1% chloroauric acid treatment Room temperature (MPa) High temperature (MPa) (150℃) 1 1.03 0.75 2 1.56 1.03 3 0.97 1.56 4 1.23 1.64 5 1.15 1.23 6 1.63 1.34 average value 1.26 1.26
[0094] Table 10 Tensile shear strength of gold printed circuit board and aluminum plate in comparative example 3 at room temperature and high temperature
[0095] 15% Thiol Treatment Room temperature (MPa) High temperature (MPa) (150℃) 1 2.56 2.17 2 3.12 2.20 3 1.88 2.09 4 2.12 1.88 5 1.52 1.79 6 1.63 1.90 average value 2.14 2.01
[0096] It can be seen from Tables 1 to 10 that, under room temperature conditions, compared with Comparative Example 1, the tensile shear strength between the surface-modified gold printed circuit board and the aluminum plate in Examples 1 to 7 of the present invention is significantly improved, and the specific improvement is shown in Table 11. This is because the chloroauric acid solution and the thiol solution are rapidly oxidized and reduced on the surface of the gold printed circuit board, changing the microscopic morphology of the surface of the gold printed circuit board, and some gold atoms are deposited and adsorbed on the gold surface to become active sites, forming Au-S covalent bonds with the active group thiol in the thiol, and the affinity between the surface modification layer of the surface-modified gold printed circuit board and the cyanate adhesive is improved, and finally the tensile shear strength of the surface-modified gold printed circuit board-cyanate adhesive film-aluminum plate shear specimen is further improved, and the bonding strength between the gold printed circuit board and the common cyanate adhesive is significantly increased, so that the gold printed circuit board and the adhesive have a better bonding effect.
[0097] From Tables 1 to 10, it can be seen that the bonding strength between the surface-modified gold printed circuit board and the aluminum plate in Example 2 (thiol solution concentration of 15% and gold chlorate solution of 1%) is the best. It should be noted that for Examples 1 to 5, the only difference between them is the concentration of the thiol solution. Compared with Example 1 (when the concentration of the thiol solution is less than 15%), as the concentration of the thiol solution in Example 2 increases, the number of active groups increases, the physical connection gradually turns into a covalent bond connection, and the bonding strength between the surface-modified gold printed circuit board and the aluminum plate becomes higher and higher; compared with Examples 3 to 5 (when the concentration of the thiol solution is greater than 15%), the bonding strength between the surface-modified gold printed circuit board and the aluminum plate is improved. This is because as the concentration of the thiol solution continues to increase, the viscosity of the solution increases, which reduces the wettability of the thiol and the gold surface, thereby affecting the bonding strength of the gold surface.
[0098] Under high temperature conditions, the results are similar to those at room temperature. Compared with Comparative Example 1, the shear strength of the surface modified gold printed circuit board-cyanate ester film-aluminum plate shear specimens in Examples 1 to 7 of the present invention is significantly improved. It can be seen that the surface modified gold obtained by treating with the gold surface modifier of the present invention can meet the bonding requirements under conventional conditions and also meet the bonding requirements under extreme environments.
[0099] Table 11 Enhancement of tensile shear strength of surface modified gold printed circuit boards and aluminum plates obtained in Examples 1 to 7 at room temperature and high temperature compared with that of Comparative Example 1
[0100] Room temperature (%) High temperature (%) (150℃) Example 1 263 301 Example 2 465 538 Example 3 419 503 Example 4 360 363 Example 5 121 121 Example 6 432 445 Example 7 387 416
[0101] Compared with Example 2, Comparative Examples 2 and 3 do not use gold chlorate solution and thiol solution together as gold surface modifiers. Comparative Example 2 only uses a gold chlorate solution with a concentration of 1wt% as a gold surface modifier; Comparative Example 3 only uses a thiol solution with a concentration of 15wt% as a gold surface modifier. Compared with Comparative Example 2, at room temperature, the shear strength between the surface-modified gold printed circuit board and the aluminum plate in Example 2 increases by 380%; at high temperature, the shear strength between the surface-modified gold printed circuit board and the aluminum plate in Example 2 increases by 351%. Compared with Comparative Example 3, at room temperature, the shear strength between the surface-modified gold printed circuit board and the aluminum plate in Example 2 increases by 183%; at high temperature, the shear strength between the surface-modified gold printed circuit board and the aluminum plate in Example 2 increases by 183%. It can be seen that the synergistic effect of gold chlorate solution and thiol solution ultimately significantly enhances the shear strength between the surface-modified gold printed circuit board and the aluminum plate, that is, significantly improves the bonding strength between the gold surface and other materials.
[0102] In summary, the gold surface is modified by the gold surface modifier of the present invention, and then coated with an adhesive to form a gold-thiol-adhesive gradient structure, which enhances the affinity between the gold surface and the adhesive; at the same time, the active group thiol is introduced into the surface of the gold, so that the gold surface can react to form a covalent bond, significantly improving the bonding strength between the gold surface and other materials. The gold surface modifier of the present invention can increase the bonding strength between gold and the adhesive through a simple chemical reaction at room temperature and pressure. At the same time, the use of the gold surface modifier will neither cause irreversible damage to the gold surface nor rely on a large number of large equipment. The process is simple, the conditions are loose, the raw materials are easy to obtain, and the reaction is rapid. It can be used on a large scale industrially and is widely used in electronic, aerospace and other technical fields. In addition, the surface-modified gold obtained by the gold surface modifier of the present invention can meet the bonding requirements under extreme environments.
Claims
1. A gold surface modifier, Features: The gold surface modifier comprises a chloroauric acid solution dissolved in a first solvent and a thiol solution dissolved in a second solvent.
2. The gold surface modifier according to claim 1, Features: The thiol is a multi-arm thiol, preferably a two-arm thiol; and / or The first solvent is anhydrous ethanol; and / or The second solvent is acetone.
3. The gold surface modifier according to claim 2, Features: The two-arm thiol is any one of 1,6-hexanedithiol, 1,5-pentanedithiol, 1,8-octanedithiol and 1,2-benzenedithiol.
4. The gold surface modifier according to claim 1, Features: The concentration of the thiol solution is 10-50 wt %, preferably 15-30 wt %.
5. The gold surface modifier according to claim 1, Features: The concentration of the chloroauric acid solution is 0.5-2 wt %, preferably 1-1.5 wt %.
6. The gold surface modifier according to claim 1, Features: The gold surface is a gold printed circuit surface.
7. A method for surface modification of gold, Features The method comprises The chloroauric acid solution described in any one of claims 1 to 6 is applied to the gold surface, reacted to obtain the first surface-modified gold; the thiol solution described in any one of claims 1 to 6 is applied to the first surface-modified gold, reacted to obtain the surface-modified gold.
8. A method for surface modification of gold, Features The method comprises The thiol solution described in any one of claims 1 to 6 is applied to the gold surface, reacted to obtain the first surface-modified gold; the chloroauric acid solution described in any one of claims 1 to 6 is applied to the first surface-modified gold, reacted to obtain the surface-modified gold.
9. The method for surface modification of gold according to claim 7 or 8, Features: The reaction time is 5 to 10 minutes.
10. Surface modified gold obtained by the surface modification method according to any one of claims 7 to 9.
Citation Information
Cited By
Gold surface anticoagulant coating structure as well as preparation method and application thereof
CN119424767A
A gold surface anticoagulant coating structure and a preparation method and application thereof
CN119424767B