Method for synthesizing carbon fiber loaded copper-cobalt-silver ternary alloy catalyst through carbon thermal shock and application of carbon fiber loaded copper-cobalt-silver ternary alloy catalyst
Preparation of carbon fiber-supported copper-cobalt silver ternary alloy catalysts through carbon thermal shock method, solving the problems of high energy consumption and insufficient active sites in traditional ammonia synthesis technology, and achieving efficient and stable electrocatalytic nitrate conversion, with wide applications prospect.
Patent Information
- Application Number
- CN202411061108.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-05
- Publication Date
- 2024-11-19
AI Technical Summary
Traditional Haber-Boschage synthesis of ammonia has high energy consumption and large CO2 emissions. The electrocatalytic nitrogen reduction synthesis of ammonia faces the problems of ammonia production rate and low Faraday efficiency. Metal copper, as an electrocatalytic nitrate ammonia production catalyst, has insufficient active sites.
The carbon fiber-loaded copper-cobalt silver ternary alloy catalyst was synthesized by carbon thermal shock method, using carbon paper, water and ethanol as solvents, spraying the metal precursor solution, infrared drying and Joule heating, to achieve a rapid carbon thermal shock process, and prepare high Active and stable catalyst.
Achieve efficient and stable ammonia yield and Faraday efficiency in electrocatalytic nitrate conversion. The Faraday efficiency reaches 93.72%, and the ammonia yield is 279.88 μmol/h/cm2, which simplifies the preparation process, reduces costs, and has a broad range of Practical application prospects.
Smart Images

Figure CN118979273A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of preparation of electrocatalytic nitrate to ammonia catalyst, and specifically relates to a method for carbon thermal shock synthesis of carbon fiber-loaded copper-cobalt-silver ternary alloy catalyst and application of the catalyst in electrocatalytic nitrate to ammonia conversion. Background Art
[0002] Ammonia (NH3), as an important inorganic chemical product, plays a vital role in the national economy. Ammonia is not only an important raw material for the chemical industry, but also a carbon-free energy carrier and a safe hydrogen storage medium. At present, the main method for synthesizing ammonia in industry is the Haber-Bosch Process, which uses nitrogen and hydrogen to react under high temperature, high pressure and in the presence of a catalyst to produce ammonia. Since its advent in the early 20th century, this process has become the mainstream technology for synthesizing ammonia worldwide. However, the traditional Haber-Bosch process has problems such as high energy consumption and large CO2 emissions. Therefore, it is crucial to develop a sustainable and efficient ammonia production technology that can be conveniently coupled with clean energy.
[0003] In recent years, electrocatalytic nitrogen reduction to ammonia and electrocatalytic nitrate reduction to ammonia have gradually become research hotspots. Electrocatalytic nitrogen reduction to ammonia is a new type of ammonia synthesis technology driven by electrical energy and using green and environmentally friendly H2O and N2 as raw materials. This method is expected to replace the traditional Haber-Bosch process and achieve energy-saving and green production of ammonia. However, due to the high inertness of nitrogen molecules and the strong N≡N bond, electrocatalytic nitrogen reduction still faces technical challenges in terms of ammonia production rate and Faraday efficiency. Therefore, electrochemical reduction of nitrate to ammonia (NO3RR) is an ideal choice, because the bond energy of the N=O bond in the nitrate is low (204kJ / mol) and the theoretical reaction potential is high (0.69Vvs.RHE), which makes it easier to electrocatalyze nitrate to ammonia. NO3RR uses nitrate ions that are widely present in water bodies as a nitrogen source to achieve ammonia synthesis through electrocatalytic reduction reaction. This method can not only effectively treat nitrate pollution in water bodies, but also simultaneously generate high-value-added ammonia products, with significant environmental and economic benefits.
[0004] At present, many metals (Cu, Zn, Ni, Fe, etc.) have been explored for the electro-reduction of nitrate to ammonia system, among which copper has shown excellent electro-catalytic reduction of nitrate. However, copper metal has insufficient active sites as a catalyst for electro-catalytic nitrate to ammonia production. The problem of insufficient active sites in the electro-catalytic nitrate to ammonia production reaction can be adjusted by introducing alloying strategies. The carbon thermal shock method (CTS) has the advantage of fast heating rate, which can achieve high temperature heating above 3000K, and can achieve rapid heating and cooling of samples by controlling the reaction time. This method can prepare multi-element alloys containing a variety of different metal elements by rapid heating and cooling of metal precursors on oxidized carbon carriers. The multi-element alloys synthesized by CTS have a narrow size distribution and are uniformly dispersed on the carbon carrier. During the CTS process, the high temperature plus the catalytic activity of the liquid metal promotes rapid particle "fission" and "fusion", resulting in uniform mixing of multiple elements. Subsequently, the rapid cooling rate promotes the kinetic control of the thermodynamic mixing region and can form crystalline solid solution nanoparticles or nanosheets. Based on this, the present invention reduces the copper ions, cobalt ions and silver ions in the solution into a copper-cobalt-silver ternary alloy supported on carbon fibers through a simple one-step carbon thermal shock (CTS) method for use in a reaction system for electrocatalytic reduction of nitrate to ammonia. There are currently no related reports in this regard. Summary of the invention
[0005] The technical problem solved by the present invention is to provide a method for synthesizing a carbon fiber-supported copper-cobalt-silver ternary alloy catalyst by carbon thermal shock, which has a simple process, low cost and excellent performance. The method uses carbon fiber paper as a substrate, water and ethanol as solvents, and prepares a precursor solution composed of copper nitrate trihydrate, cobalt nitrate hexahydrate and silver nitrate metal salt in a certain proportion. The carbon fiber-supported copper-cobalt-silver ternary alloy catalyst is successfully synthesized by carbon thermal shock technology. The catalyst shows excellent catalytic activity and stability in electrocatalytic nitrate ammonia conversion.
[0006] The present invention adopts the following technical solution to solve the above technical problems, a method for carbon thermal shock synthesis of carbon fiber loaded with copper-cobalt-silver ternary alloy catalyst, characterized in that the specific steps are: Step S1: cutting the carbon paper and performing surface cleaning treatment to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate, cobalt nitrate hexahydrate and silver nitrate with a total metal ion molar concentration of 0.3 mol / L to obtain a metal precursor solution A; Step S3: spray the metal precursor solution A obtained in step S2 onto the carbon paper obtained in step S1 with a spray gun, and ensure that the metal precursor solution A completely covers the carbon paper, and then place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B; Step S4: placing the material B obtained in step S3 in a Joule heating device and continuously introducing argon gas, maintaining the vacuum degree at 1.2~1.4Mpa when introducing argon gas, ensuring that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides, setting the carbon thermal shock temperature to 1000~1200°C and the carbon thermal shock time to 6~10s to achieve a rapid carbon thermal shock process to obtain a carbon fiber-supported copper-cobalt-silver ternary alloy catalyst, which exhibits excellent catalytic activity and stability in electrocatalytic nitrate transamination.
[0007] It is further defined that the molar ratio of copper ions, cobalt ions and silver ions in the metal precursor solution A in step S2 is 2:0.5:0.5, and the solvent is a mixed solution of water and ethanol in a volume ratio of 1:1.
[0008] It is further defined that the carbon thermal shock temperature in step S3 is 1100° C., the mode is selected as the program control mode, and the specific parameter settings are respectively the current is 19A and the time is 8s.
[0009] The invention discloses an application of the carbon fiber-supported copper-cobalt-silver ternary alloy catalyst in electrocatalytic nitrate transamination. The catalyst exhibits excellent nitrate transamination catalytic activity and stability in electrocatalytic nitrate transamination, with a Faradaic efficiency of 93.72% and an ammonia yield of 279.88 μmol / h / cm 2 .
[0010] Compared with the prior art, the present invention has the following advantages and beneficial effects: 1. The carbon thermal shock method preparation process involved in the present invention is simple, time-saving and efficient, and avoids the complex processes such as high-temperature pyrolysis and hydrothermal reaction involved in the conventional preparation of nitrate transamination catalysts. Through the rapid heating and cooling process, the reaction between metal elements can be quickly activated to promote the formation of alloy phases, thereby greatly shortening the preparation cycle and improving production efficiency. The present invention uses cheap and readily available copper nitrate trihydrate, cobalt nitrate hexahydrate, and silver nitrate as metal precursor salts, and a highly active carbon fiber-supported copper-cobalt-silver alloy nitrate transamination electrocatalyst can be obtained by a simple carbon thermal shock method, and the method has the potential for large-scale production.
[0011] 2. The present invention successfully obtained a copper-cobalt-silver ternary alloy catalyst by regulating the reaction temperature and time during the carbon thermal shock process. The copper-cobalt-silver ternary alloy prepared by the present invention exhibits excellent nitrate reduction activity under neutral conditions, with a Faradaic efficiency of 93.72% and an ammonia yield of 279.88 μmol / h / cm 2 , and the invention shows good stability during continuous operation, indicating that the alloy catalyst has broad practical application prospects in the field of nitrate transamination. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is a scanning electron microscope image of the product C1 prepared in Example 1; Figure 2 X-ray diffraction patterns of products C1-C4 prepared in Example 1 and Comparative Examples 1-3; Figure 3 This is the full X-ray photoelectron spectrum of the product C1 prepared in Example 1; Figure 4 The linear sweep voltammetry curves of the nitrate transamination catalysts of the products C1-C4 prepared in Example 1 and Comparative Examples 1-3; Figure 5 The linear sweep voltammetry curves of the product C1 prepared in Example 1 in pure K2SO4 and K2SO4 + KNO3 solutions; Figure 6 The product C1 prepared in Example 1 shows the Faraday efficiency and ammonia yield of nitrate to ammonia at different potentials during the NO3RR process; Figure 7 The Faradaic efficiency and ammonia yield of nitrate to ammonia conversion of product C1 prepared in Example 1 during the stability test; Figure 8 This is a graph showing the ammonia yield of product C1 prepared in Example 1 in pure K2SO4 and K2SO4 + KNO3 solutions. DETAILED DESCRIPTION
[0013] The above contents of the present invention are further described in detail below through examples, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following examples, and all technologies implemented based on the above contents of the present invention belong to the scope of the present invention. Example 1
[0014] Step S1: cutting the carbon paper into a rectangle of a required size (1 cm×9 cm), and performing surface cleaning to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate, cobalt nitrate hexahydrate and silver nitrate with a total metal ion molar concentration of 0.3 mol / L, wherein the molar ratio of copper ion, cobalt ion and silver ion is 2:0.5:0.5, to obtain a metal precursor solution A1; Step S3: Take out 1 mL of the metal precursor solution A1 obtained in step S2, spray it on the carbon paper obtained in step S1 with a 0.3 mm spray gun, ensure that the metal precursor solution A1 completely covers the carbon paper, and place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B1; Step S4: placing the material B1 obtained in step S3 in a Joule heating device and continuously introducing argon gas; maintaining the vacuum degree at 1.2-1.4 MPa when introducing argon gas; ensuring that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides; setting the carbon thermal shock temperature (1100°C) and time (8s) to achieve a rapid carbon thermal shock process to obtain the carbon fiber-supported copper-cobalt-silver ternary alloy catalyst C1.
[0015] Comparative Example 1 Step S1: cutting the carbon paper into a rectangle of a required size (1 cm×9 cm), and performing surface cleaning to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate and silver nitrate with a total metal ion molar concentration of 0.3 mol / L, wherein the molar ratio of copper ions to silver ions is 2:0.5, to obtain a metal precursor solution A2; Step S3: Take out 1 mL of the metal precursor solution A2 obtained in step S2, spray it on the carbon paper obtained in step S2 with a 0.3 mm spray gun, ensure that the metal precursor solution A2 completely covers the carbon paper, and place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B2; Step S4: Place the material B2 obtained in step S3 in a Joule heating device and continuously introduce argon gas. When introducing argon gas, maintain the vacuum degree at 1.2~1.4Mpa to ensure that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides. Set the temperature (1100°C) and time (8s) of the carbon thermal shock to achieve a rapid carbon thermal shock process to obtain material C2.
[0016] Comparative Example 2 Step S1: cutting the carbon paper into a rectangle of a required size (1 cm×9 cm), and performing surface cleaning to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate and cobalt nitrate hexahydrate with a total metal ion molar concentration of 0.3 mol / L, wherein the molar ratio of copper ions to cobalt ions is 2:0.5, to obtain a metal precursor solution A3; Step S3: Take out 1 mL of the metal precursor solution A3 obtained in step S2, spray it on the carbon paper obtained in step S1 with a 0.3 mm spray gun, ensure that the metal precursor solution A3 completely covers the carbon paper, and place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B3; Step S4: Place the material B3 obtained in step S3 in a Joule heating device and continuously introduce argon gas. When introducing argon gas, maintain the vacuum degree at 1.2~1.4Mpa to ensure that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides. Set the temperature (1100°C) and time (8s) of the carbon thermal shock to achieve a rapid carbon thermal shock process to obtain material C3.
[0017] Comparative Example 3 Step S1: cutting the carbon paper into a rectangle of a required size (1 cm×9 cm), and performing surface cleaning to remove surface impurities; Step S2: preparing a copper nitrate trihydrate solution having a total metal ion molar concentration of 0.3 mol / L to obtain a metal precursor solution A4; Step S3: Take out 1 mL of the metal precursor solution A4 obtained in step S2, spray it on the carbon paper obtained in step S1 with a 0.3 mm spray gun, ensure that the metal precursor solution A4 completely covers the carbon paper, and place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B4; Step S4: Place the material B4 obtained in step S3 in a Joule heating device and continuously introduce argon gas. When introducing argon gas, maintain the vacuum degree at 1.2~1.4Mpa to ensure that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides. Set the temperature (1100°C) and time (8s) of the carbon thermal shock to achieve a rapid carbon thermal shock process to obtain material C4.
[0018] NO3RR activity test process: The prepared NO3RR electrocatalyst (C1 / C2 / C3 / C4) was placed in a Pt sheet electrode holder as a working electrode, a saturated calomel electrode (SCE) was used as a reference electrode, a Pt sheet was used as a counter electrode, and a 0.5 mol / L K2SO4+0.1mol / L KNO3 mixed aqueous solution was used as an electrolyte to form a three-electrode test system. The LSV test was performed to obtain the LSV polarization curves of the C1-C4 catalysts, with a scan rate of 5mV / s and a potential range of -0.6~-1.6V; a chronoamperometric response test was performed in a 0.5mol / L K2SO4 + 0.1mol / LKNO3 mixed solution to obtain the chronoamperometric curves of the C1 catalyst at different potentials, with a reaction time of 1800s. The electrolytes under different catalysts were tested for indophenol blue using a UV-visible spectrophotometer, and their UV-visible spectroscopic curves were finally obtained.
[0019] The product C1 prepared in Example 1 showed excellent nitrate transamination activity and stability as an electrocatalyst in nitrate transamination, with a Faradaic efficiency of 93.72% and an ammonia yield of 279.88 μmol / h / cm 2 , and the invention shows good stability during continuous operation, indicating that the alloy catalyst has broad practical application prospects in the field of nitrate transamination.
[0020] The above embodiments describe the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions are only for illustrating the principles of the present invention. Without departing from the scope of the principles of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of protection of the present invention.
Claims
1. A method for synthesizing carbon fiber loaded with copper-cobalt-silver ternary alloy catalyst by carbon thermal shock, characterized in that The specific steps are: Step S1: cutting the carbon paper and performing surface cleaning to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate, cobalt nitrate hexahydrate and silver nitrate with a total metal ion molar concentration of 0.3 mol / L to obtain a metal precursor solution A; Step S3: spray the metal precursor solution A obtained in step S2 onto the carbon paper obtained in step S1 with a spray gun, and ensure that the metal precursor solution A completely covers the carbon paper, and then place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B; Step S4: placing the material B obtained in step S3 in a Joule heating device and continuously introducing argon gas, maintaining the vacuum degree at 1.2~1.4Mpa when introducing argon gas, ensuring that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides, setting the carbon thermal shock temperature to 1000~1200°C and the carbon thermal shock time to 6~10s to achieve a rapid carbon thermal shock process to obtain a carbon fiber-supported copper-cobalt-silver ternary alloy catalyst, which exhibits excellent catalytic activity and stability in electrocatalytic nitrate transamination.
2. The method for carbon thermal shock synthesis of carbon fibers loaded with copper-cobalt-silver ternary alloy catalyst according to claim 1, characterized in that: In step S2, the molar ratio of copper ions, cobalt ions and silver ions in the metal precursor solution A is 2:0.5:0.5, and the solvent is a mixed solution of water and ethanol in a volume ratio of 1:
1.
3. The method for carbon thermal shock synthesis of carbon fibers loaded with copper-cobalt-silver ternary alloy catalyst according to claim 1, characterized in that: The carbon thermal shock temperature in step S3 is 1100° C., the mode is selected as the program control mode, and the specific parameter settings are the current of 19A and the time of 8s.
4. The method for synthesizing carbon fiber by carbon thermal shock and supporting copper-cobalt-silver ternary alloy catalyst according to claim 1, characterized in that The specific steps are: Step S1: cutting the carbon paper into a rectangle of the required size of 1 cm×9 cm, and performing surface cleaning treatment to remove surface impurities; Step S2: preparing a mixed solution of copper nitrate trihydrate, cobalt nitrate hexahydrate and silver nitrate with a total metal ion molar concentration of 0.3 mol / L, wherein the molar ratio of copper ion, cobalt ion and silver ion is 2:0.5:0.5, to obtain a metal precursor solution A; Step S3: Take out 1 mL of the metal precursor solution A obtained in step S2, spray it on the carbon paper obtained in step S1 with a 0.3 mm spray gun, ensure that the metal precursor solution A completely covers the carbon paper, and place it under an infrared lamp until the surface of the carbon paper is completely dry to obtain material B; Step S4: placing material B obtained in step S3 in a Joule heating device and continuously introducing argon gas; maintaining the vacuum degree at 1.2-1.4 MPa when introducing argon gas to ensure that there is no air residue in the cavity of the Joule heating device to avoid the generation of oxides; setting the carbon thermal shock temperature to 1100°C and the carbon thermal shock time to 8s to achieve a rapid carbon thermal shock process to obtain a carbon fiber-supported copper-cobalt-silver ternary alloy catalyst.
5. Application of the carbon fiber-supported copper-cobalt-silver ternary alloy prepared by the method according to claim 4 in electrocatalytic nitrate transamination, the catalyst exhibits excellent nitrate transamination catalytic activity and stability, the Faraday efficiency reaches 93.72%, and the ammonia yield is 279.88 μmol / h / cm 2 .