NF / rGO / Co-Ni-S / Mo-O self-supporting composite material and preparation method and application thereof
By growing NF/rGO and Co-Ni-S/Mo-O core-shell structures on nickel foam, combined with the active sites of graphene oxide, the preparation complexity and stability of non-precious metal catalysts in electrocatalytic hydrogen evolution are solved. Problem, efficient catalyst performance and long life are achieved.
Patent Information
- Application Number
- CN202411068577.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-06
- Publication Date
- 2024-11-19
AI Technical Summary
In the electrocatalytic hydrogen evolution process, existing non-precious metal catalysts have problems such as complex preparation process, low content of active substances, easy catalyst fall off and poor stability, especially self-supporting materials with smooth surfaces are prone to agglomeration.
Using foam nickel as the first carrier, using its good conductivity and three-dimensional network structure to grow NF/rGO as a self-supporting framework, and then the Co-Ni-S/Mo-O core-shell structure is grown on its surface by hydrothermal method. The abundant active sites and morphological characteristics of reducing graphene oxide are used to form a putaway structure to improve the stability and activity of the catalyst.
The preparation process is simplified, the stability and electrochemical active area of the catalyst are improved, the catalyst shedding and agglomeration are reduced, and the hydrogen evolution performance and service life are significantly improved.
Smart Images

Figure CN118979277A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electrocatalytic hydrogen evolution, and in particular to a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material and a preparation method and application thereof. Background Art
[0002] Precious metal Pt and platinum-based hydrogen evolution catalysts have good electrical conductivity and high catalytic activity. However, precious metal materials are scarce and expensive. At the same time, precious metal catalysts are susceptible to corrosion under strong acid or strong base conditions, which reduces their lifespan. Therefore, the common solution is to use non-precious metals as hydrogen evolution catalysts. However, non-precious metal hydrogen evolution catalysts have low catalytic activity and poor stability.
[0003] In order to solve the problem of poor catalytic performance of non-precious metal catalysts due to limited catalytic active sites, the hydrogen evolution performance can be improved by regulating its composition, structure and surface properties. For example, the existing document 1 (An B, Dong J, Su H, et al. Electron redistributed vanadium anchored CoFe phosphides as effective electrocatalysts for boosting overall water splitting [J]. International Journal of Hydrogen Energy, 2023.) uses cobalt nitrate hexahydrate, potassium ferrocyanide, sodium citrate, and ammonium metavanadate as raw materials, and obtains V-CoFe PBA by a mixing and stirring method, and then uses sodium hypophosphite as a raw material to obtain V-CoFeP by tubular furnace annealing. This technical solution obtains excellent hydrogen evolution catalytic performance at a current density of 10 mA cm -2 Under the condition of , the overpotential is only 53mV. However, since V-CoFeP is a powder catalyst, Nafion solution needs to be used as a binder to make V-CoFeP into a V-CoFeP / GC electrode for hydrogen evolution reaction. That is, this technical solution has the problems of complex process and low content of active substances.
[0004] In order to solve the problems of complex process and poor operability of powdered non-precious metal hydrogen evolution catalysts, the active material can be directly grown on a conductive substrate to form a self-supporting material to solve the problem caused by the need to use a binder. For example, the existing document 2 (Lv Z, Zhong D, Zang M, et al. Boosting alkaline hydrogen evolution via spontaneous built-in electric field [J]. Rare Metals, 2024.) uses nickel foam as a substrate, cobalt nitrate hexahydrate, sodium metavanadate, ammonium fluoride and urea as raw materials, and prepares VCo-OH NFs@NF by a hydrothermal method, and then uses sodium hypophosphite as a raw material to obtain VCo-PN NFs@NF by tubular furnace annealing. This technical solution achieves good hydrogen evolution catalytic performance at a current density of 10 mA cm -2 Under the condition of , the overpotential is only 51mV. However, since the VCo-PN NFs@NF nanowires are in direct contact with the electrolyte during the hydrogen evolution reaction, there is a problem of partial detachment of the catalyst after a long reaction time, which leads to a significant decrease in stability. That is, this technical solution cannot solve the problem of poor stability.
[0005] In order to solve the problem of poor stability of self-supporting non-precious metal hydrogen evolution catalysts, a core-shell structure can be constructed, and the shell material can be used as a protective layer to prevent the core material from falling off and being oxidized. For example, the existing document 3 (Liu S, XanH, Song Z, et al. Interface engineering of multi-component phosphide / sulfide core-shell heterostructure for efficient overall water splitting [J]. International Journal of Hydrogen Energy, 2024.) uses nickel foam as a substrate, nickel nitrate hexahydrate, ferrous sulfate heptahydrate and sodium molybdate as raw materials, and obtains Fe-NiMoO4 by a hydrothermal method, and then uses phosphorus powder as a raw material to obtain FeNiP-NiMoO by annealing. x Then, FeNiP-NiMoO was prepared by electrodeposition using cobalt sulfate hexahydrate, sodium chloride, boric acid, thiourea and trisodium citrate as raw materials. x @CoNiS. This technical solution achieved excellent hydrogen evolution catalytic performance at a current density of 10 mA cm -2Under the condition of , the overpotential is only 67.5mV. However, since this technical solution directly uses nickel foam as the supporting material, the relatively smooth surface of nickel foam causes the active material to easily agglomerate, thereby reducing the catalyst active sites, that is, this technical solution has a serious agglomeration problem.
[0006] Unlike self-supporting materials with relatively smooth surfaces, such as nickel foam, reduced graphene oxide has abundant active sites that can anchor the catalyst on the surface; in addition, reduced graphene oxide also has the function of regulating the morphology and microstructure of the catalyst. For example, the existing document 4 (Sun A, Qiu Y, Chen K, et al. Constructing built-in electric field in oxygen vacancies-enriched Fe3O4-FeSe2 heterojunctions supported on reduced graphene oxide for efficient overall water splitting [J]. Journal of Colloid and Interface Science, 2024.) uses urea, ferric nitrate nonahydrate, ammonium fluoride, and graphene oxide dispersion as raw materials to prepare Fe3O4 / GO by a hydrothermal method, and then uses selenium powder and sodium borohydride as raw materials to obtain Fe3O4-FeSe2 / rGO by a hydrothermal method. This technical solution has achieved excellent hydrogen evolution catalytic performance at a current density of 100 mA cm -2 Under the condition of , the overpotential is 234 mV. However, using reduced graphene oxide as a carrier, only powdered catalysts can be obtained, that is, the aforementioned technical problem of requiring the use of a binder also exists.
[0007] Therefore, when non-precious metal catalysts are used as electrocatalytic hydrogen evolution materials, the technical problems that must be solved are: the preparation process is complex, the content of active substances is low; the catalyst is easy to fall off and the stability is poor; and the self-supporting material with a smooth surface is prone to agglomeration. To solve the above problems, we can start from the following three aspects:
[0008] 1. Use self-supporting catalyst materials to replace powdered catalysts, simplify the preparation process and reduce the loss of active substances;
[0009] 2. Construct a core-shell structure and utilize the protective effect of the shell structure to reduce material shedding and improve the stability of the catalyst;
[0010] 3. By selecting suitable self-supporting materials, we can utilize the rich active sites and morphology-regulating characteristics of reduced graphene oxide and combine it with self-supporting materials with smooth surfaces to anchor the catalyst on its surface and reduce the occurrence of agglomeration. Summary of the invention
[0011] The purpose of the present invention is to provide a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material and a preparation method and application thereof.
[0012] According to the inventors' research, nickel foam has good electrical conductivity and a three-dimensional network structure, and can be used as the first carrier to directly grow other electrode materials on its surface to form a self-supporting material. The self-supporting material prepared based on this principle has the advantages of a simple preparation process and a high content of active substances.
[0013] Reduced graphene oxide has abundant active sites, which can further regulate the microscopic morphology of the catalyst and reduce the occurrence of agglomeration. Based on this principle, the self-supporting material prepared allows the catalyst to grow evenly on its surface and has a larger electrochemical active area.
[0014] In the core-shell structure, the shell structure fully plays a protective role, enabling the core structure to maximize its catalytic activity. The self-supporting core-shell structure material prepared based on this principle has greatly reduced material shedding, thereby improving the stability of the catalyst and extending its service life.
[0015] Therefore, the present invention uses nickel foam as the first carrier and reduced graphene oxide as the second carrier to build a core-shell structure. Through a simple preparation process, the microscopic morphology is regulated, the occurrence of catalyst shedding and agglomeration is reduced, the hydrogen evolution performance of the catalyst is improved, and its service life is extended.
[0016] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is:
[0017] A NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, which uses nickel foam as a substrate, graphene oxide dispersion and ascorbic acid as raw materials, and rGO is loaded on the surface of the composite material by a water bath method to obtain NF / rGO, and then cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride are used as raw materials to obtain NF / rGO / Co-Ni-O by a hydrothermal method, and then ammonium molybdate tetrahydrate and thiourea are used as raw materials to grow Co-Ni-S / Mo-O on the surface of NF / rGO by a two-step hydrothermal method to obtain NF / rGO / Co-Ni-S / Mo-O;
[0018] The NF / rGO serves as a self-supporting skeleton; the microscopic morphology of the MoO2 is a nano-sheet structure; the microscopic morphology of the CoNi2S4 is a micron-sheet structure, wherein MoO2 is coated on the surface of CoNi2S4, and the two form a shell-core structure, wherein the shell structure is composed of MoO2 and the core structure is composed of CoNi2S4.
[0019] A method for preparing a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material comprises the following steps:
[0020] Step 1, preparation of NF / rGO, first, graphene oxide dispersion and deionized water are mixed, and then ultrasonicated under certain conditions to obtain solution A; then, ascorbic acid is added to solution A and fully dispersed under ultrasonic conditions to obtain solution B; finally, under certain conditions, the washed nickel foam NF is immersed in solution B for water bathing, and after the water bathing, it is washed and dried to obtain reduced graphene oxide-coated nickel foam, referred to as NF / rGO;
[0021] In the step 1, the method for washing the nickel foam is to wash the nickel foam with acetone, hydrochloric acid, deionized water and anhydrous ethanol in sequence, and then dry it after washing;
[0022] In the step 1, the ultrasonic condition for preparing solution A is that the ultrasonic time is 0.5-1h;
[0023] The mass ratio of graphene oxide dispersion and ascorbic acid was 3:20;
[0024] In the step 1, the conditions for preparing solution B are to add under ultrasonic conditions, and the ascorbic acid is added in two times;
[0025] In step 1, the water bath conditions are: the water bath temperature is 85-95° C., and the water bath time is 6-8 hours;
[0026] Step 2, preparation of NF / rGO / Co-Ni-O, first, cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride are dissolved in deionized water in a certain mass ratio to obtain a C solution; then, under certain conditions, the NF / rGO obtained in step 1 is immersed in the C solution for a hydrothermal reaction, and after the hydrothermal reaction is completed, the reduced graphene oxide-coated nickel foam loaded with cobalt nickel oxide is obtained by washing and drying, referred to as NF / rGO / Co-Ni-O;
[0027] In the step 2, the mass ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride is 3:2:3:1;
[0028] In step 2, the conditions of the hydrothermal reaction are: the hydrothermal temperature is 110-130° C., and the hydrothermal time is 6-8 h;
[0029] Step 3, preparation of NF / rGO / Co-Ni-S / Mo-O, dissolving ammonium molybdate tetrahydrate and urea in deionized water to obtain a D solution; then, under certain conditions, immersing the NF / rGO / Co-Ni-O obtained in step 2 in the D solution for a hydrothermal reaction, washing and drying after the hydrothermal reaction, to obtain a reduced graphene oxide-coated nickel foam loaded with cobalt nickel sulfide and molybdenum oxide, i.e., a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, referred to as NF / rGO / Co-Ni-S / Mo-O;
[0030] In step 1, step 2 and step 3, the immersion method is vertical immersion;
[0031] In the step 3, the mass ratio of ammonium molybdate tetrahydrate to thiourea is 12:11;
[0032] In step 3, the conditions of the hydrothermal reaction are: the hydrothermal temperature is 190-210° C., and the hydrothermal time is 12-13 h.
[0033] A NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, when used as a hydrogen evolution catalyst material, reacts in 1M KOH solution, in the range of 0 to -0.1V, when the current density is 10mA·cm -2 When the overpotential is 65mV, the Tafel slope is 96.48mV·dec -1 , after 136h of it test, the current retention rate was 98%.
[0034] The technical effects of the present invention have been tested experimentally, and the specific contents are as follows:
[0035] The XRD test of the present invention shows that NF / rGO / Co-Ni-S / Mo-O has characteristic peaks of CoNi2S4 and MoO2 at the same time. The test results are compared with step 2, and it can be seen that step 3 successfully prepares MoO2, that is, NF / rGO / Co-Ni-S / Mo-O is successfully prepared.
[0036] TEM and EDS tests show that the present invention successfully synthesizes uniformly distributed CoNi2S4 and MoO2 in NF / rGO / Co-Ni-S / Mo-O, and MoO2 nanosheets grow uniformly on the surface of CoNi2S4, that is, in a core-shell structure, the core structure is composed of CoNi2S4, and the shell structure is composed of MoO2.
[0037] The SEM test of the present invention shows that nano-sheet MoO2 grows on the surface of sheet-like CoNi2S4.
[0038] The electrochemical performance test of the present invention shows that: in 1M KOH solution, in the range of 0 to -1.0V, when the current density is 10mA·cm -2 When NF / rGO / Co-Ni-S / Mo-O has an overpotential of 65 mV, the Tafel slope is 96.48 mV·dec -1 , after 136h of it test, the current retention rate was 98%.
[0039] Therefore, the present invention has the following advantages over the prior art:
[0040] 1. When constructing the NF / rGO / Co-Ni-S / Mo-O composite catalyst, nickel foam is used as the first carrier. While retaining its good conductive properties, a self-supporting material is prepared, solving the problem of complex preparation process of ordinary powdered catalysts.
[0041] 2. When constructing the NF / rGO / Co-Ni-S / Mo-O composite catalyst, reduced graphene oxide is used as the second carrier material to coat the surface of nickel foam. While using its abundant active sites to anchor the catalyst on the surface, it also achieves the regulation of catalyst morphology and micromorphology, reduces agglomeration, and increases the active sites of Co-Ni-S / Mo-O.
[0042] 3. In the NF / rGO / Co-Ni-S / Mo-O composite catalyst, a unique core-shell structure is formed between the Co-Ni-S / Mo-O loaded on the conductive substrate. The shell structure protects the core structure, reduces the problem of core material falling off, enables its catalytic activity to be fully exerted, and also greatly improves the stability of the catalyst and prolongs its service life;
[0043] 4. NF / rGO / Co-Ni-S / Mo-O has good electrocatalytic hydrogen evolution performance. The catalyst has both synergistic effects between the carrier and the active substance and synergistic effects between different phases. The existence of this effect enhances their original hydrogen evolution catalytic activity and realizes the design of "1+1>2". BRIEF DESCRIPTION OF THE DRAWINGS
[0044] Figure 1 It is the XRD test pattern of Example 1;
[0045] Figure 2 The XRD test diagrams of Comparative Example 1, Comparative Example 2 and Comparative Example 3 are shown;
[0046] Figure 3 It is the XRD test pattern of comparative example 4;
[0047] Figure 4This is the SEM test image of NF / rGO / Co-Ni-O prepared in Example 1;
[0048] Figure 5 This is the SEM test image of NF / rGO / Co-Ni-S / Mo-O prepared in Example 1;
[0049] Figure 6 This is the SEM test image of NF / Co-Ni-S / Mo-O prepared in Comparative Example 1;
[0050] Figure 7 This is the SEM test image of NF / rGO / Mo-O prepared in Comparative Example 2;
[0051] Figure 8 This is the SEM test image of NF / rGO / Co-Ni-S prepared in Comparative Example 3;
[0052] Fig. 9 This is the SEM test image of NF / rGO / Co-Ni-S / Mo-OH prepared in Comparative Example 4;
[0053] Fig.10 TEM test image of NF / rGO / Co-Ni-S / Mo-O prepared in Example 1;
[0054] Fig.11 This is the EDS image of NF / rGO / Co-Ni-S / Mo-O prepared in Example 1;
[0055] Fig.12 is the LSV diagram of Example 1;
[0056] Fig.13 LSV diagrams of comparative example 1, comparative example 2, and comparative example 3;
[0057] Fig.14 is the LSV diagram of Comparative Example 4;
[0058] Fig.15 The Tafel diagrams are Example 1, Comparative Example 1, Comparative Example 2, and Comparative Example 3;
[0059] Fig.16 It is the Tafel diagram of Comparative Example 4;
[0060] Fig.17 This is the IT stability test diagram of Example 1. DETAILED DESCRIPTION
[0061] The present invention is further described in detail through embodiments and in conjunction with the accompanying drawings, but the present invention is not limited thereto.
[0062] Example 1
[0063] A method for preparing a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material comprises the following steps:
[0064] Step 1, preparation of NF / rGO, first, 5 mL of 6 g / L graphene oxide dispersion and 30 mL of deionized water are mixed, and then ultrasonicated for 30 min to obtain solution A; then, under ultrasonic conditions, 0.2 g of ascorbic acid is added to solution A twice to fully disperse, to obtain solution B; finally, under the conditions of a water bath temperature of 90°C and a water bath time of 6 h, the washed nickel foam NF is vertically immersed in solution B for water bathing, and after washing and drying, reduced graphene oxide-coated nickel foam, referred to as NF / rGO, is obtained;
[0065] In the step 1, the method for washing the nickel foam is to wash the nickel foam with acetone, hydrochloric acid, deionized water and anhydrous ethanol in sequence, and after washing, dry the nickel foam at a drying temperature of 60° C.
[0066] Step 2, preparation of NF / rGO / Co-Ni-O, first, dissolving 0.582 g of cobalt nitrate hexahydrate, 0.436 g of nickel nitrate hexahydrate, 0.6 g of urea and 0.185 g of ammonium fluoride in 60 mL of deionized water to obtain a C solution; then, vertically immersing the NF / rGO obtained in step 1 into the C solution for a hydrothermal reaction at a hydrothermal temperature of 120° C. for a hydrothermal time of 6 h, washing and drying after the hydrothermal reaction to obtain reduced graphene oxide-coated nickel foam loaded with cobalt nickel oxide, referred to as NF / rGO / Co-Ni-O;
[0067] In order to verify the composition of the obtained NF / rGO / Co-Ni-O, XRD test was performed. The test results are shown in Figure 1 As shown, NF / rGO / Co-Ni-O has characteristic peaks of Co2NiO4. The test results show that step 2 successfully prepared Co2NiO4, that is, NF / rGO / Co-Ni-O was successfully prepared.
[0068] In order to verify the microstructure of NF / rGO / Co-Ni-O, SEM test was performed. The test results are shown in Figure 4 As shown, Co2NiO4 is a flake structure, and at the same time, the Co2NiO4 flake structure is coated on the surface of NF / rGO.
[0069] In order to prove the electrochemical performance of NF / rGO / Co-Ni-O, electrochemical performance tests were carried out. The specific method of the electrochemical performance test is to conduct electrochemical performance tests in a three-electrode system consisting of the material to be tested as the working electrode, the mercuric oxide electrode as the reference electrode, the graphite electrode as the counter electrode, and 1M KOH solution as the electrolyte. The test results are shown in Figure 2. Fig.12 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2 When , the overpotential of NF / rGO / Co-Ni-O is 215 mV;
[0070] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.15 As shown in Figure 2, the Tafel slope of NF / rGO / Co-Ni-O is 101.7 mV·dec -1 .
[0071] Step 3, preparation of NF / rGO / Co-Ni-S / Mo-O, dissolving 0.247 g of ammonium molybdate tetrahydrate and 0.228 g of thiourea in 50 mL of deionized water to obtain a D solution; then, vertically immersing the NF / rGO / Co-Ni-O obtained in step 2 into the D solution for a hydrothermal reaction at a hydrothermal temperature of 200 ° C and a hydrothermal time of 12 h, washing and drying after the hydrothermal reaction to obtain reduced graphene oxide-coated nickel foam loaded with cobalt nickel sulfide and molybdenum oxide, i.e., a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, referred to as NF / rGO / Co-Ni-S / Mo-O.
[0072] In order to prove the composition of NF / rGO / Co-Ni-S / Mo-O, XRD test was carried out. The test results are shown in Figure 1 As shown, NF / rGO / Co-Ni-S / Mo-O has characteristic peaks of CoNi2S4 and MoO2 at the same time. The test results show that step 3 successfully prepared MoO2, that is, NF / rGO / Co-Ni-S / Mo-O was successfully prepared.
[0073] In order to further prove the composition of NF / rGO / Co-Ni-S / Mo-O, TEM test and EDS test were carried out.
[0074] TEM test results are as follows Fig.10 As shown, the lattice fringe spacing of 0.272nm matches the (222) crystal plane of CoNi2S4, and the lattice fringe spacing of 0.218nm matches the (101) crystal plane of MoO2, and NF / rGO / Co-Ni-S / Mo-O has a core-shell structure. The test results show that NF / rGO / Co-Ni-S / Mo-O successfully synthesizes CoNi2S4 and MoO2.
[0075] EDS test results are as follows Fig.11 As shown, Ni, Co, S, Mo, and O elements are evenly distributed on the surface of the material.
[0076] Through the combination of TEM and EDS tests, it can be seen that NF / rGO / Co-Ni-S / Mo-O successfully synthesized uniformly distributed CoNi2S4 and MoO2, and MoO2 nanosheets grew uniformly on the surface of CoNi2S4, that is, in a core-shell structure, the core structure is composed of CoNi2S4 and the shell structure is composed of MoO2.
[0077] In order to verify the microstructure of NF / rGO / Co-Ni-S / Mo-O, SEM test was carried out. The test results are shown in Figure 5 As shown, a nanosheet structure has newly grown on the surface of the sheet-like CoNi2S4. Combined with the XRD test results, it can be seen that the component of the nanosheet structure is MoO2, referred to as MoO2 nanosheet.
[0078] Further combined with the SEM test results of NF / rGO / Co-Ni-O obtained in step 2, it can be seen that NF / rGO / Co-Ni-S / Mo-O has a core-shell structure, in which the inner layer structure is composed of CoNi2S4 and the outer layer structure is composed of MoO2 nanosheets.
[0079] In order to prove the electrochemical performance of NF / rGO / Co-Ni-S / Mo-O, the electrochemical catalytic performance test was carried out. The test results are shown in Fig.12 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2 When the overpotential of NF / rGO / Co-Ni-S / Mo-O is 65mV, it can be seen from the comparison with step 2 that under the same conditions, the overpotential of NF / rGO / Co-Ni-S / Mo-O is significantly reduced, which indicates that the MoO2 synthesized in step 3 and the CoNi2S4 generated by sulfidation have a synergistic effect, which can significantly reduce the overpotential.
[0080] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.15 As shown in Figure 2, the Tafel slope of NF / rGO / Co-Ni-S / Mo-O is 96.48 mV·dec -1 Compared with step 2, under the same conditions, the Tafel slope of NF / rGO / Co-Ni-S / Mo-O decreases, indicating that the CoNi2S4-MoO2 core-shell structure prepared by step 3 can accelerate the charge transfer rate, that is, increase the reaction rate and reduce the Tafel slope.
[0081] In order to prove the stability of NF / rGO / Co-Ni-S / Mo-O, stability performance test was carried out. The test results are shown in Fig.17 As shown, the current density is 10 mA cm -2, the current retention rate is 98% under the condition of a cycle time of 136h. The test results show that the NF / rGO / Co-Ni-S / Mo-O self-supporting composite material has good stability.
[0082] In order to prove the role of each component, namely rGO, MoO2 and CoNi2S4, in the technical solution, comparative examples 1, 2 and 3 are provided, which are respectively:
[0083] Comparative Example 1 is that rGO is not introduced, that is, step 1 is not performed, and CoNi2S4 and MoO2 are directly grown on NF in sequence;
[0084] Comparative Example 2 is that CoNi2S4 is not introduced, that is, MoO2 is directly grown on the NF / rGO obtained in step 1;
[0085] Comparative Example 3 is that MoO2 is not introduced, that is, only CoNi2S4 is prepared on the NF / rGO / Co-Ni-O obtained in step 2.
[0086] Comparative Example 1
[0087] A method for preparing NF / Co-Ni-S / Mo-O, wherein the steps not particularly described in the specific steps are the same as the preparation method of Example 1, except that: step 1 is not required, and in step 2, NF is used instead of NF / rGO, and the obtained material is named NF / Co-Ni-S / Mo-O.
[0088] In order to prove the composition of NF / Co-Ni-S / Mo-O, XRD test was carried out. The test results are shown in Figure 2 As shown, NF / Co-Ni-S / Mo-O has characteristic peaks of CoNi2S4 and MoO2 at the same time. The test results show that CoNi2S4 and MoO2 are successfully prepared, that is, NF / Co-Ni-S / Mo-O is successfully prepared.
[0089] The SEM test results of NF / Co-Ni-S / Mo-O are as follows Figure 6 As shown, although MoO2 still maintains a nano-sheet structure, the microstructure of CoNi2S4 is a rod-like structure. Compared with Example 1, it can be seen that the introduction of rGO changes the microstructure of CoNi2S4 from a rod-like structure to a sheet-like structure.
[0090] The electrochemical performance test results of NF / Co-Ni-S / Mo-O are as follows Fig.13 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2When , the overpotential of NF / Co-Ni-S / Mo-O is 72mV. Compared with Example 1, it can be seen that the introduction of rGO significantly improves the conductivity of the catalyst, that is, accelerates the transmission of electrons on the catalyst surface;
[0091] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.15 As shown, the Tafel slope of NF / Co-Ni-S / Mo-O is 277.57 mV·dec -1 Compared with Example 1, it can be seen that the introduction of rGO can increase the active sites of the catalyst, and after being compounded with CoNi2S4, the electrochemical active area can be increased, and activation is achieved when hydrogen ions are adsorbed, that is, activated hydrogen ions are obtained, thereby reducing the energy barrier of the hydrogen evolution reaction and accelerating the rate of the hydrogen evolution reaction.
[0092] By comparing Example 1 with Comparative Example 1, it can be seen that rGO is introduced as a carrier template to form flaky CoNi2S4, increase the effective reaction area, and improve the hydrogen evolution performance. The reason is that the unique structure of rGO provides sufficient active sites for the growth of CoNi2S4, inducing the conversion of rod-shaped CoNi2S4 into flaky CoNi2S4.
[0093] Comparative Example 2
[0094] A method for preparing NF / rGO / Mo-O, wherein the steps not particularly described in the specific steps are the same as the preparation method of Example 1, except that: step 2 is not required, and in step 3, thiourea is not required to be added, and the obtained material is named NF / rGO / Mo-O.
[0095] In order to prove the composition of NF / rGO / Mo-O, XRD test was carried out. The test results are shown in Figure 2 As shown, NF / rGO / Mo-O has characteristic peaks of MoO2. The test results show that MoO2 is successfully prepared, that is, NF / rGO / Mo-O is successfully prepared.
[0096] The SEM test results of NF / rGO / Mo-O are as follows Figure 7 As shown, MoO2 still maintains a nanosheet structure, but the MoO2 nanosheets are in a disordered and scattered state, and there is agglomeration. Compared with Example 1, it can be seen that the introduction of CoNi2S4 makes the MoO2 nanosheets evenly distributed in the sheet-like CoNi2S4.
[0097] The electrochemical performance test results of NF / rGO / Mo-O are shown in Fig.13 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2When , the overpotential of NF / rGO / Mo-O is 148mV. Compared with Example 1, it can be seen that the introduction of CoNi2S4 can reduce the energy barrier of the reaction. The reason is that CoNi2S4 has a unique electronic structure, which is conducive to the adsorption and reduction of hydrogen ions. In addition, after the composite of CoNi2S4 and MoO2, the catalytic performance is further improved through synergistic effect.
[0098] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.15 As shown in Figure 2, the Tafel slope of NF / rGO / Mo-O is 198.17 mV·dec -1 Compared with Example 1, it can be seen that the introduction of CoNi2S4 can improve the electrical contact between the catalyst and the electrode, thereby reducing the electron transfer resistance and ultimately achieving an increase in the hydrogen evolution reaction rate.
[0099] By comparing Example 1 and Comparative Example 2, it can be seen that the introduction of the CoNi2S4 flaky structure allows the originally dispersed MoO2 nanosheets to grow evenly dispersed on its surface, effectively improving the hydrogen evolution catalytic activity. The reason is that the flaky CoNi2S4 provides a large number of active sites for the growth of MoO2 nanosheets, reduces the occurrence of agglomeration, and increases the effective contact area between MoO2 and the electrolyte. At the same time, there is a synergistic effect between the two.
[0100] Comparative Example 3
[0101] A method for preparing NF / rGO / Co-Ni-S, wherein the steps not specifically described are the same as those of the preparation method of Example 1, except that in step 3, ammonium molybdate tetrahydrate does not need to be added, and the obtained material is named NF / rGO / Co-Ni-S.
[0102] In order to prove the composition of NF / rGO / Co-Ni-S, XRD test was carried out. The test results are shown in Figure 2 As shown, NF / rGO / Co-Ni-S has the characteristic peak of CoNi2S4. The test results show that CoNi2S4 is successfully prepared, that is, NF / rGO / Co-Ni-S is successfully prepared.
[0103] The SEM test results of NF / rGO / Co-Ni-S are as follows Figure 8 As shown, CoNi2S4 agglomerates into a block structure. Compared with Example 1, it can be seen that the introduction of MoO2 changes the microstructure of CoNi2S4 from a block structure to a flake structure.
[0104] The electrochemical performance test results of NF / rGO / Co-Ni-S are shown in Fig.13 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2When , the overpotential of NF / rGO / Co-Ni-S is 156mV. Compared with Example 1, it can be seen that the introduction of MoO2 can improve the oxygen affinity of the catalyst and promote the dissociation of water, thereby accelerating the hydrogen evolution reaction process. Moreover, after MoO2 is composited with CoNi2S4, the catalytic activity of the hydrogen evolution reaction can be significantly improved.
[0105] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.15 As shown in Figure 2, the Tafel slope of NF / rGO / Co-Ni-S is 114.9 mV·dec -1 Compared with Example 1, it can be seen that the introduction of MoO2 can improve the charge transfer ability inside the catalyst, thereby reducing the energy barrier of the hydrogen evolution reaction and improving the hydrogen evolution performance of the catalyst.
[0106] By comparing Example 1 with Comparative Example 3, it can be seen that the introduction of MoO2 nanosheet structure can effectively control the morphology, increase the effective contact area between the catalyst and the electrolyte, and improve the hydrogen evolution catalytic performance. The reason is that MoO2 can reduce the agglomeration phenomenon. At the same time, there is a synergistic effect with CoNi2S4, and the core-shell structure formed between the two accelerates the charge transfer.
[0107] In order to demonstrate the influence of the immersion method on the technical effect, comparative example 4 is provided, which is a NF / rGO / Co-Ni-S / Mo-O prepared by horizontal immersion.
[0108] Comparative Example 4
[0109] A preparation method of NF / rGO / Co-Ni-S / Mo-O based on horizontal immersion, wherein the steps not particularly specified in the specific steps are the same as the preparation method of Example 1, except that: in all steps, horizontal immersion is used instead of vertical immersion, that is, the NF in step 1, the NF / rGO in step 2, and the NF / rGO / Co-Ni-O in step 3 are all operated accordingly by horizontal immersion, and the obtained material is named NF / rGO / Co-Ni-S / Mo-OH.
[0110] In order to prove the composition of NF / rGO / Co-Ni-S / Mo-OH, XRD test was carried out. The test results are shown in Figure 3 As shown, NF / rGO / Co-Ni-S / Mo-OH only has obvious NF characteristic peaks, and the characteristic peaks of rGO, CoNi2S4 and MoO2 diffraction crystal planes are not obvious. The test results show that rGO and CoNi2S4-MoO2 cannot be loaded on NF in large quantities, that is, NF / rGO / CoNi2S4-MoO2-H was not successfully prepared.
[0111] The SEM test results of NF / rGO / Co-Ni-S / Mo-OH are as follows Fig. 9 As shown, the NF surface presents a feather-like structure, and no other structures appear. The test results show that rGO, CoNi2S4, and MoO2 cannot be loaded on NF in large quantities, that is, NF / rGO / CoNi2S4-MoO2 was not successfully prepared.
[0112] The electrochemical performance test results of NF / rGO / Co-Ni-S / Mo-OH are as follows Fig.14 As shown, in the range of 0 to -1.0 V, at a current density of 10 mA cm -2 When , the overpotential of NF / rGO / Co-Ni-S / Mo-OH is 175mV. Compared with Example 1, vertical immersion makes the sample surface more fully contact with the solution, thereby improving the growth uniformity and efficiency of the composite material;
[0113] The Tafel slope can be calculated by current polarization test. The test results are as follows: Fig.16 As shown in Figure 2, the Tafel slope of NF / rGO / Co-Ni-S / Mo-OH is 228.2 mV·dec -1 Compared with Example 1, vertical immersion reduces excessive aggregation and decomposition of reactants in local areas, thereby reducing the possibility of impurity generation.
[0114] By comparing Example 1 and Comparative Example 4, it can be seen that horizontal immersion causes NF to float on the surface of the solution, resulting in rGO, CoNi2S4, and MoO2 only growing on one side of the NF surface, ultimately resulting in a significant decrease in the electrocatalytic hydrogen evolution performance. Therefore, Example 1 and Comparative Example 4 show that the immersion method has a significant impact on the performance of the material.
[0115] The following conclusions can be drawn from the above Example 1, Comparative Example 1, Comparative Example 2, Comparative Example 3, and Comparative Example 4:
[0116] 1. Multi-element transition metal sulfides have sufficient active sites and a large exposed area, which provide a large number of sites for the growth of MoO2, making it evenly dispersed and growing on the surface, reducing the occurrence of agglomeration. The synergistic effect between the two also improves the catalytic activity of the catalyst;
[0117] 2. As a carrier template, rGO has excellent conductivity and chemical stability, which accelerates the transmission of electrons on the catalyst surface. Its unique structure provides sufficient active sites, increases the effective reaction area, and accelerates the rate of hydrogen evolution reaction;
[0118] 3. As a transition metal oxide, MoO2 has a unique crystal structure with good conductivity and chemical stability, which can effectively regulate the morphology of CoNi2S4 and improve the catalytic performance of hydrogen evolution. MoO2 nanosheets are loaded on the surface of flaky CoNi2S4. The core-shell structure formed between the two not only improves the stability of the catalyst, but also gives full play to the synergistic effect between different components.
[0119] 4. Different immersion methods of the material have a significant impact on the hydrogen evolution performance. Vertically immersing the sample in the reaction solution can make the catalyst grow evenly and dispersedly on the surface of the nickel foam. The uniform growth of the catalyst also ensures its electrocatalytic hydrogen evolution performance.
Claims
1. A NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, characterized in that: Using nickel foam as a substrate, graphene oxide dispersion and ascorbic acid as raw materials, rGO is loaded on its surface by a water bath method to obtain NF / rGO, and then cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride are used as raw materials to obtain NF / rGO / Co-Ni-O by a hydrothermal method. Then, ammonium molybdate tetrahydrate and thiourea are used as raw materials to grow Co-Ni-S / Mo-O on the surface of NF / rGO by a two-step hydrothermal method, and finally NF / rGO / Co-Ni-S / Mo-O is obtained.
2. The NF / rGO / Co-Ni-S / Mo-O self-supporting composite material according to claim 1, characterized in that: The NF / rGO serves as a self-supporting skeleton; the microscopic morphology of the MoO2 is a nano-sheet structure; the microscopic morphology of the CoNi2S4 is a micron-sheet structure, wherein MoO2 is coated on the surface of CoNi2S4, and the two form a shell-core structure, wherein the shell structure is composed of MoO2 and the core structure is composed of CoNi2S4.
3. A method for preparing a NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, characterized in that The following steps are involved: Step 1, preparation of NF / rGO, first, graphene oxide dispersion and deionized water are mixed, and then ultrasonicated under certain conditions to obtain solution A; then, ascorbic acid is added to solution A and fully dispersed under ultrasonic conditions to obtain solution B; finally, under certain conditions, the washed nickel foam NF is immersed in solution B for water bathing, and after the water bathing, it is washed and dried to obtain reduced graphene oxide-coated nickel foam, referred to as NF / rGO; Step 2, preparation of NF / rGO / Co-Ni-O, first, cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride are dissolved in deionized water in a certain mass ratio to obtain a C solution; then, under certain conditions, the NF / rGO obtained in step 1 is immersed in the C solution for a hydrothermal reaction, and after the hydrothermal reaction is completed, the reduced graphene oxide-coated nickel foam loaded with cobalt nickel oxide is obtained by washing and drying, referred to as NF / rGO / Co-Ni-O; Step 3, preparation of NF / rGO / Co-Ni-S / Mo-O, dissolving ammonium molybdate tetrahydrate and urea in deionized water to obtain solution D; then, under certain conditions, immersing the NF / rGO / Co-Ni-O obtained in step 2 in solution D for hydrothermal reaction, washing and drying after the hydrothermal reaction, to obtain reduced graphene oxide-coated nickel foam loaded with cobalt nickel sulfide and molybdenum oxide, that is, NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, referred to as NF / rGO / Co-Ni-S / Mo-O.
4. The preparation method according to claim 3, characterized in that: The mass ratio of the graphene oxide dispersion to ascorbic acid is 3:20; In the step 2, the mass ratio of cobalt nitrate hexahydrate, nickel nitrate hexahydrate, urea and ammonium fluoride is 3:2:3:1; In the step 3, the mass ratio of ammonium molybdate tetrahydrate to thiourea is 12:
11.
5. The preparation method according to claim 3, characterized in that: In the step 1, the method for washing the nickel foam is to wash the nickel foam with acetone, hydrochloric acid, deionized water and anhydrous ethanol in sequence, and then dry it after washing; In step 1, step 2 and step 3, the immersion method is vertical immersion.
6. The preparation method according to claim 3, characterized in that: In the step 1, the ultrasonic condition for preparing solution A is that the ultrasonic time is 0.5-1h; In the step 1, the conditions for preparing solution B are to add under ultrasonic conditions, and the ascorbic acid is added in two times; In step 1, the water bath conditions are as follows: the water bath temperature is 85-95° C., and the water bath time is 6-8 h.
7. The preparation method according to claim 3, characterized in that: In the step 2, the conditions of the hydrothermal reaction are: the hydrothermal temperature is 110-130° C., and the hydrothermal time is 6-8 hours.
8. The preparation method according to claim 3, characterized in that: In step 3, the conditions of the hydrothermal reaction are: the hydrothermal temperature is 190-210° C., and the hydrothermal time is 12-13 h.
9. A NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, characterized in that: When used as a hydrogen evolution catalyst material, the reaction is carried out in a 1M KOH solution, and the current density is 10 mA cm in the range of 0 to -0.1 V. -2 When the overpotential is 65mV, the Tafel slope is 96.48mV·dec -1 .
10. A NF / rGO / Co-Ni-S / Mo-O self-supporting composite material, characterized in that: When used as a hydrogen evolution catalyst material, the current retention rate is 98% after 136 hours of IT testing.
Citation Information
Cited By
Preparation method and application of fluorine-doped Co2NiO4 (at) RGO three-dimensional heterostructure electrode material and sodium ion battery
CN121641971A
A method for preparing a fluorine-doped Co2NiO4@RGO three-dimensional heterostructure electrode material, its application, and a sodium-ion battery.