Carbon-doped gallium arsenide polycrystal, preparation method thereof and equipment for preparing carbon-doped gallium arsenide polycrystal

By using a carbon-doped gallium arsenide polycrystalline method, the problems of large resistance differences and high dislocation density in traditional methods have been solved, resulting in improved uniformity of carrier concentration and resistivity, reduced dislocation density, and increased production efficiency.

CN118979306APending Publication Date: 2024-11-19VITAL MICRO-ELECTRONICS TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411083683.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing technologies make it difficult to fabricate semi-insulating gallium arsenide single crystals with low dislocation density and uniform electrical properties. Traditional methods result in large resistance differences, which affect the electrical performance of the devices.

Method used

Carbon-doped gallium arsenide polycrystalline material was prepared by controlling the carbon concentration at (0.2~2)×1015 atoms/cm3, using hollow cylindrical carbon-doped gallium arsenide polycrystalline material as raw material, combined with the vertical gradient condensation method, and controlling the flow rates of carbon monoxide and hydrogen.

Benefits of technology

It significantly improves the uniformity of carrier concentration and resistivity, reduces dislocation density, and enhances the electrical performance uniformity and production efficiency of gallium arsenide single crystals.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004984545120000111
    Figure BDA0004984545120000111
  • Figure HDA0004984545130000011
    Figure HDA0004984545130000011
  • Figure HDA0004984545130000012
    Figure HDA0004984545130000012
Patent Text Reader

Abstract

The invention discloses a carbon-doped gallium arsenide polycrystal, a preparation method of the carbon-doped gallium arsenide polycrystal and equipment for preparing the carbon-doped gallium arsenide polycrystal, and belongs to the technical field of materials. The carbon concentration of the carbon-doped gallium arsenide polycrystal is (0.2-2) * 10 < 15 > atoms / cm < 3 >; the carbon-doped gallium arsenide polycrystal has a hollow cylinder structure; the outer diameter of the hollow cylinder structure is 76-150mm, and the inner diameter of the hollow cylinder structure is 10-20mm; the height of the hollow cylinder structure ranges from 200 mm to 400 mm. The carbon-doped gallium arsenide polycrystal has high carrier concentration and resistivity and good electrical property uniformity, and the gallium arsenide single crystal with uniform electrical property distribution and small dislocation density can be prepared by using the carbon-doped gallium arsenide polycrystal as a raw material of the gallium arsenide single crystal. According to the preparation method of the carbon-doped gallium arsenide polycrystal, the production efficiency of the gallium arsenide polycrystal is remarkably improved, and the weight of the gallium arsenide polycrystal is increased by more than 100% under a one-time preparation process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of material technology, and in particular to a carbon-doped gallium arsenide polycrystal and a preparation method thereof, and equipment for preparing the carbon-doped gallium arsenide polycrystal. Background Art

[0002] Gallium arsenide (GaAs) single crystals have become a very important basic material for microelectronics and optoelectronics, used to manufacture optoelectronic devices such as lasers, detectors, red light LEDs, and ultra-high-speed digital integrated circuits and high-frequency microwave and millimeter-wave devices for network optical communications. Low-resistance (SC) GaAs single crystals are required to make optoelectronic devices, while high-quality semi-insulating (SI) GaAs wafers are required as substrates to make ultra-high-speed digital circuits and high-frequency microwave power devices. This is because, on the one hand, the purity of GaAs materials is far from reaching the level of elemental semiconductors Si and Ge, and on the other hand, GaAs has a chemical ratio deviation problem during high-temperature growth, which can lead to intrinsic point defects such as vacancies, interstitials, and anti-sites and produce their complexes. Therefore, ordinary GaAs cannot meet the preparation requirements of the above-mentioned optoelectronic devices, ultra-high-speed digital circuits, and high-frequency microwave power devices.

[0003] In addition, the above-mentioned vacancies and anti-site defects are electrically active, which participate in the electrical compensation of the material and change during the subsequent heat treatment process, thereby affecting the quality of the material. Although the ideal intrinsic GaAs single crystal is semi-insulating, its production process is complicated and difficult to achieve. Therefore, almost all SI-GaAs (semi-insulating gallium arsenide) is obtained through electrical compensation. At present, SI-GaAs used in microelectronics is mainly achieved by controlling the mutual compensation of an intrinsic deep defect EL2 with an energy level located in the center of the bandgap and the acceptor impurity C. However, the control of defects and electrical compensation is often complicated, so the common method of obtaining SI-GaAs by electrical compensation has the disadvantages of high dislocation density and low crystallization rate.

[0004] The vertical gradient solidification method (VGF) is a crystal growth method in which a container containing materials is placed vertically at a corresponding temperature gradient position set in a furnace. After the materials are fully melted, they slowly crystallize from the lower end and continue to the upper end. Compared with the high-pressure liquid-sealed Czochralski method (LEC), these two methods have great differences in chemical ratio deviation, C doping and content control during the growth of SI-GaAs single crystals. In addition, the number and concentration of deep energy level defects of VGF-SI-GaAs single crystals (SI-GaAs single crystals generated by the VGF method) will be different from those of LEC-SI-GaAs single crystals (SI-GaAs single crystals generated by the LEC method), and the electrical compensation and performance of the VGF-SI-GaAs single crystals are different from those of the LEC-SI-GaAs single crystal materials. In addition, the dislocation density of the VGF-SI-GaAs single crystal and the dislocations extending from the substrate to the epitaxial layer are significantly reduced, which has a certain impact on the performance and life of microwave devices. Therefore, it has become a focus of attention to obtain excellent electrical properties by regulating the deep energy level defects and electrical compensation of VGF-SI-GaAs single crystals.

[0005] The traditional high steric hindrance VGF-SI-GaAs single crystal growth uses undoped high-purity 7N gallium arsenide polycrystalline material as raw material, melts the polycrystalline material by high-temperature heating, adds carbon caps to make the C doping evaporated at high temperature fuse into the gallium arsenide polycrystalline solution, and produces high steric hindrance semi-insulating gallium arsenide single crystals by vertical gradient condensation. Although this growth method can obtain low-dislocation VGF-SI-GaAs single crystals, due to the uneven distribution of C doping in the gallium arsenide polycrystalline solution at high temperature, the lateral resistance difference of the gallium arsenide polycrystalline is very large, and then the resistivity difference of the VGF-SI-GaAs single crystal prepared from the gallium arsenide polycrystalline in the same horizontal plane wafer can reach more than 100%. In severe cases, the resistance difference of the VGF-SI-GaAs single crystal will cause a cliff-like failure of the device electrical performance.

[0006] Therefore, in order to prepare SI-GaAs single crystals with low dislocation density and uniform electrical properties, it is of great significance to study and develop a method for preparing VGF-SI-GaAs polycrystals with semi-insulating properties. Summary of the invention

[0007] In view of this, the technical problem to be solved by the present invention is to provide a carbon-doped gallium arsenide polycrystal and a preparation method thereof, and an apparatus for preparing the carbon-doped gallium arsenide polycrystal. The carbon-doped gallium arsenide polycrystal has a high carrier concentration and resistivity and good performance uniformity.

[0008] In order to achieve the above purpose, the technical solution adopted by the present invention is as follows:

[0009] The present invention provides a carbon-doped gallium arsenide polycrystal, wherein the carbon concentration is (0.2-2)×1015 atoms / cm 3 ;

[0010] The carbon-doped gallium arsenide polycrystal has a hollow cylindrical structure;

[0011] Preferably, the outer diameter of the hollow cylindrical structure is 76-150 mm, and the inner diameter is 10-20 mm; more preferably, the outer diameter of the hollow cylindrical structure is 76-100 mm, and the inner diameter is 10-15 mm; further preferably, the outer diameter of the hollow cylindrical structure is 76-85 mm, and the inner diameter is 10-13 mm.

[0012] Preferably, the carbon concentration of the carbon-doped gallium arsenide polycrystal is (0.5-1.5)×10 15 atoms / cm 3 ; More preferably (0.8~1.2)×10 15 atoms / cm 3 .

[0013] In some specific embodiments of the present invention, the outer diameter of the hollow cylindrical structure is 76 mm and the inner diameter is 10 mm.

[0014] Preferably, the height of the hollow cylindrical structure is 200-400 mm; more preferably, the height of the hollow cylindrical structure is 300-350 mm.

[0015] The carbon-doped gallium arsenide polycrystal of the present invention has higher carrier concentration and resistivity.

[0016] Preferably, in the present invention, the sum of other impurities in the carbon-doped gallium arsenide polycrystal is less than 100 PPB.

[0017] The remaining impurities include but are not limited to elemental impurities such as Fe, Zn, and Ca.

[0018] Preferably, the carrier concentration of the carbon-doped gallium arsenide polycrystal is (1-60)×10 6 cm 3 More preferably, the carrier concentration of the carbon-doped gallium arsenide polycrystal is (1.5-50)×10 6 cm 3 .

[0019] Preferably, the average carrier concentration of the head of the carbon-doped gallium arsenide polycrystal is (1.5-4)×10 6 cm 3 In some specific embodiments of the present invention, the average carrier concentration of the head of the carbon-doped gallium arsenide polycrystal is 2.18×10 6 cm 3 or 1.84×106 cm 3 or 2.06×10 6 cm 3 or 3.43 × 10 6 cm 3 ;

[0020] Preferably, the average carrier concentration of the tail of the carbon-doped gallium arsenide polycrystal is (3-7)×10 6 cm 3 In some specific embodiments of the present invention, the average carrier concentration of the tail of the carbon-doped gallium arsenide polycrystal is 3.44×10 7 cm 3 or 4.37 × 10 7 cm 3 or 4.21×10 7 cm 3 or 6.55×10 6 cm 3 .

[0021] Preferably, the resistivity of the carbon-doped gallium arsenide polycrystal is (1-10)×10 8 ohm.cm; More preferably, the resistivity of the carbon-doped gallium arsenide polycrystalline is (2 to 9)×10 8 ohm.cm.

[0022] Preferably, the average resistivity of the head of the carbon-doped gallium arsenide polycrystal is (2-4)×10 8 In some specific embodiments of the present invention, the average resistivity of the head of the carbon-doped gallium arsenide polycrystal is 2.58×10 8 ohm.cm or 2.33×10 8 ohm.cm or 2.44×10 8 ohm.cm or 3.12×10 8 ohm.cm.

[0023] Preferably, the tail average resistivity of the carbon-doped gallium arsenide polycrystal is (5-9)×10 8 In some specific embodiments of the present invention, the average resistivity of the tail of the carbon-doped gallium arsenide polycrystal is 6.75×10 8 ohm.cm or 7.04×10 8 ohm.cm or 5.68×10 8 ohm.cm or 8.66×10 8 ohm.cm.

[0024] Due to the crystal segregation effect, the doped carbon and other impurities flow into the liquid faster than into the solid, so the average carrier concentration and the average resistivity of the tail of the carbon-doped gallium arsenide polycrystal are greater than those of the head.

[0025] The present invention also provides an apparatus for preparing the carbon-doped gallium arsenide polycrystal, comprising a polycrystal synthesis furnace and a stepped quartz tube arranged inside the polycrystal synthesis furnace;

[0026] The stepped quartz tube comprises a tube body, one end of which is open, and the other end of which is provided with a Y-shaped gas delivery pipe for delivering hydrogen and carbon monoxide;

[0027] The tube body comprises two coaxially arranged tube body units, the tube body units are in the shape of a circular tube, and the diameters of the two tube body units gradually increase from the Y-shaped gas delivery pipe to the opening;

[0028] The upper tube unit of the stepped quartz tube is provided with a quartz crucible with a hollow cone, and the lower tube unit is provided with a hollow cylindrical quartz crucible. The upper tube unit is the tube unit in the opening direction.

[0029] The hollow cylindrical quartz crucible comprises a quartz crucible with a conical bottom and a hollow cylinder arranged inside the crucible;

[0030] The top of the hollow cylinder is sealed and small holes are provided on both sides for the introduction of gas;

[0031] A quartz cap is provided on the top of the stepped quartz tube;

[0032] The top of the quartz cap is provided with a feed port for feeding or vacuuming;

[0033] The Y-shaped gas delivery pipe is provided with a ventilation pipeline valve for controlling the flow of the gas introduced. Preferably, the outer diameter of the hollow cylindrical quartz crucible is 76-150 mm, and the inner diameter is 10-20 mm;

[0034] Preferably, the length of the hollow cylindrical quartz crucible is 200-450 mm.

[0035] Preferably, the diameter of the quartz crucible with a hollow cone portion is 1.2 to 1.5 times the outer diameter of the hollow cylindrical quartz crucible; more preferably 1.3 times.

[0036] The present invention also provides a method for preparing carbon-doped gallium arsenide polycrystal, which is carried out using the above-mentioned equipment and comprises the following steps:

[0037] 1) placing liquid 7N gallium and solid 7N arsenic in a hollow cylindrical quartz crucible and a quartz crucible with a hollow cone, respectively, and then evacuating to maintain a sealed vacuum environment of the stepped quartz tube;

[0038] 2) placing the stepped quartz tube in a polycrystalline synthesis furnace, and simultaneously introducing carbon monoxide and hydrogen from the Y-shaped gas pipe of the device into the liquid 7N gallium, so that the pressure inside the stepped quartz tube is 1-1.5 MPa, and then heating until the solid 7N arsenic is vaporized, and the vaporized 7N arsenic is mixed with the liquid gallium to react, so as to obtain a gallium arsenide solution;

[0039] 3) The gallium arsenide solution is subjected to a vertical gradient condensation method to prepare the carbon-doped gallium arsenide polycrystal.

[0040] In the above preparation method, the impurity metal ions such as Fe, Zn, Ca, etc. in the gallium arsenide solution will react with hydrogen at high temperature to generate metal elements such as Fe, Zn, Ca, etc.

[0041] In addition, the carbon monoxide introduced at high temperature will also react chemically with the free Ga in GaAs to form carbon element, and the reaction equation is CO+2Ga→Ga2O3+3C.

[0042] The carbon element is mixed in a gallium arsenide solution, and the carbon-doped gallium arsenide polycrystal is obtained by a vertical gradient condensation method.

[0043] In some specific embodiments of the present invention, the step 1) is specifically as follows:

[0044] Add liquid 7N gallium into the hollow cylindrical quartz crucible from the feed port of the quartz cap; add solid 7N arsenic into the quartz crucible with a hollow cone from the feed port of the quartz cap;

[0045] Next, the feed port was vacuumed and the feed port of the quartz cap was sealed.

[0046] Then, the stepped quartz tube in the sealed state is placed in a polycrystalline synthesis furnace, and carbon monoxide and hydrogen are simultaneously introduced into the liquid 7N gallium from the Y-shaped gas pipe of the device, so that the pressure inside the stepped quartz tube is 1-1.5 MPa, and then, the solid 7N arsenic is heated to vaporize, and the vaporized 7N arsenic is mixed with the liquid gallium to react to obtain a gallium arsenide solution;

[0047] Finally, carbon-doped gallium arsenide polycrystals were prepared from gallium arsenide solution using vertical gradient condensation method.

[0048] Preferably, the specific conditions of the vertical gradient condensation method in step 4) are:

[0049] Preferably, the temperature is 1235°C to 1245°C, more preferably 1238°C to 1242°C. In some specific embodiments of the present invention, the temperature is 1238°C.

[0050] Preferably, the gradient condensation time is 16 to 24 hours, more preferably 20 to 24 hours, and in some specific embodiments of the present invention, it is 16 hours or 24 hours.

[0051] Preferably, the condensation rate is 8 to 25 mm / h, more preferably 8 to 17 mm / h. In some specific embodiments of the present invention, it is 25 mm / h, 16.7 mm / h or 8.33 mm / h.

[0052] In the above preparation method, the condensation rate of the vertical gradient condensation method will also affect the performance uniformity of the carbon-doped gallium arsenide polycrystal. A fast condensation rate will cause the head and tail uniformity of the carrier concentration and resistivity of the carbon-doped gallium arsenide polycrystal to decrease.

[0053] Preferably, in the step 3), the heating temperature is between 1240°C and 1250°C.

[0054] Preferably, the heating time is 6 to 10 hours; more preferably 6 hours or 10 hours.

[0055] Preferably, in step 1), the mass ratio of solid 7N arsenic to liquid 7N gallium is (1.1-1.5):1; more preferably (1.1-1.2):1; in some specific embodiments of the present invention, the mass ratio of solid 7N arsenic to liquid 7N gallium is 1.1:1 or 1.2:1.

[0056] The excess solid 7N arsenic reacts fully with the liquid 7N gallium, reducing the gallium-rich phenomenon.

[0057] The flow rates of carbon monoxide and hydrogen will also affect the carbon doping amount (doped carbon concentration) in the carbon-doped gallium arsenide polycrystal as well as the quality, overall performance and uniformity of the performance of the carbon-doped gallium arsenide polycrystal.

[0058] Within a certain range, an increase in the carbon monoxide flow rate increases the doped carbon concentration, and the average resistivity of the head and tail of the carbon-doped gallium arsenide polycrystal will increase.

[0059] Preferably, the flow rate of carbon monoxide in step 2) is 20-30 mL / min; more preferably 25-30 mL / min; in some specific embodiments of the present invention, preferably 20 mL / min, 25 mL / min or 30 mL / min.

[0060] Within a certain range, the increase in the flow rate of hydrogen makes it possible to reduce more impure metal ions in the gallium arsenide solution obtained in step 2), and the reduced metal element does not react with GaAs, but is free outside the GaAs solution. Through the segregation of the liquid, the elemental metal impurities will gather at the tail of the polycrystal, thereby reducing the internal impurities of the polycrystal and making the polycrystal purer, thereby improving the uniformity of the electrical properties of the carbon-doped gallium arsenide polycrystal.

[0061] Preferably, the flow rate of hydrogen in step 2) is 20-30 mL / min; more preferably 25-30 mL / min; in some specific embodiments of the present invention, preferably 25 mL / min or 30 mL / min.

[0062] Preferably, the carbon monoxide and hydrogen are introduced so that the pressure inside the stepped quartz tube is 1-1.5 MPa, more preferably 1-1.2 MPa, and preferably 1 MPa, 1.1 MPa or 1.2 MPa in some specific embodiments of the present invention.

[0063] The carbon-doped gallium arsenide polycrystal prepared by the method has uniform electrical properties and low dislocation density.

[0064] The carrier concentration and resistivity of the carbon-doped gallium arsenide polycrystal of the present invention are significantly improved compared with those of conventional gallium arsenide polycrystal not doped with carbon, and the uniformity of electrical properties is significantly improved.

[0065] The present invention also provides a gallium arsenide single crystal, which is prepared from the carbon-doped gallium arsenide polycrystal or the carbon-doped gallium arsenide polycrystal prepared by the above-mentioned preparation method.

[0066] Using the carbon-doped gallium arsenide polycrystal of the present invention to prepare a single crystal can obtain a single crystal with better uniformity of electrical properties.

[0067] Compared with the prior art, the carbon-doped gallium arsenide polycrystal provided by the present invention has a carbon concentration of (0.2-2)×10 15 atoms / cm 3 ; The carbon-doped gallium arsenide polycrystal has a hollow cylindrical structure; the outer diameter of the hollow cylindrical structure is 76-150 mm, and the inner diameter is 10-20 mm; the height of the hollow cylindrical structure is 200-400 mm. The carbon-doped gallium arsenide polycrystal has a high carrier concentration, resistivity and good uniformity of electrical properties. Using it as a raw material for gallium arsenide single crystals can prepare gallium arsenide single crystals with uniform electrical property distribution and low dislocation density. The preparation method of carbon-doped gallium arsenide polycrystals described in the present invention significantly improves the production efficiency of gallium arsenide polycrystals, and achieves an increase of more than 100% in the weight of gallium arsenide polycrystals under a one-time preparation process. BRIEF DESCRIPTION OF THE DRAWINGS

[0068] Figure 1 It is a diagram of a stepped quartz tube device containing a crucible, wherein 1-1 is a hydrogen inlet pipe, 1-2 is a carbon monoxide inlet pipe, 1-3 is a ventilation pipe valve, 1-4 is a hollow cylindrical quartz crucible, 1-5 is a quartz crucible with a hollow cone, and 1-6 is a stepped quartz tube;

[0069] Figure 2The figure is a welding device diagram of a stepped quartz tube and a quartz cap, wherein 2-1 is a quartz cap, and 2-2 is a quartz cap feed port;

[0070] Figure 3 A three-dimensional image of a hollow cylindrical quartz crucible for synthesizing gallium arsenide polycrystals;

[0071] Figure 4 The sealing diagram of the quartz tube after arsenic and gallium are loaded, wherein 3-1 is liquid 7N gallium, 3-2 is solid 7N arsenic, and 3-3 is the welding point of the quartz cap feed port;

[0072] Figure 5 This is a diagram of a gallium arsenide polycrystal synthesis device, wherein 4-1 is a quartz support tube, 4-2 is a heater, and 4-3 is a polycrystal synthesis furnace. DETAILED DESCRIPTION

[0073] In order to further illustrate the present invention, a synthesis method of gallium arsenide polycrystal and gallium arsenide polycrystal provided by the present invention are described in detail below in conjunction with embodiments.

[0074] The following embodiments are described in detail Figure 1-5 The device shown is used to prepare carbon-doped gallium arsenide polycrystals.

[0075] The carbon-doped gallium arsenide polycrystal device comprises a polycrystal synthesis furnace (shown in 4-3) and a stepped quartz tube arranged inside the polycrystal synthesis furnace;

[0076] The stepped quartz tube is fixed in the polycrystalline synthesis furnace through the quartz support tube shown in 4-1;

[0077] Wherein, the stepped quartz tube comprises a tube body (shown in 1-6), one end of the tube body is open, and the other end is provided with a Y-shaped gas pipe for conveying hydrogen and carbon monoxide;

[0078] The tube body comprises two coaxially arranged tube body units, the tube body units are in the shape of a circular tube, and the diameters of the two tube body units gradually increase from the Y-shaped gas delivery pipe to the opening;

[0079] The lower part (lower tube unit) of the stepped quartz tube is provided with the hollow cylindrical quartz crucible shown in 1-4, and the upper part (upper tube unit) is provided with the quartz crucible with a hollow cone shown in 1-5, and the upper tube unit is the tube unit in the opening direction;

[0080] The hollow cylindrical quartz crucible comprises a quartz crucible with a conical bottom and a hollow cylinder arranged inside the crucible;

[0081] The top of the hollow cylinder is sealed and small holes are provided on both sides for the introduction of gas;

[0082] In the Y-shaped gas transmission pipe, 1-1 is a hydrogen inlet pipe, 1-2 is a carbon monoxide inlet pipe, and 1-3 is a ventilation pipe valve for controlling the flow of the inlet gas.

[0083] A quartz cap (shown in 2-1) is arranged on the top of the stepped quartz tube, and a feed port (shown in 2-2) is arranged on the top of the quartz cap, and the feed port is used for feeding and vacuuming.

[0084] Example 1

[0085] Step 1: Place a hollow cylindrical quartz crucible with a diameter of 76 mm and a length of 450 mm in the lower part of the stepped quartz tube, and place a quartz crucible with a conical hollow part with a diameter of 100 mm in the upper part of the stepped quartz tube;

[0086] Step 2: The quartz cap and the quartz tube are vertically welded together with an oxyhydrogen flame to make the quartz tube and the quartz cap sealed and connected;

[0087] Step 3: Pour 5 kg of liquid 7N gallium into the hollow cylindrical quartz crucible, and put 5.5 kg of solid 7N arsenic into the hollow quartz crucible, and then vacuum weld and seal the quartz cap feed port.

[0088] Step 4: Place the welded quartz tube into the polycrystalline synthesis furnace, and simultaneously input CO and H2 from the gas pipe at the bottom of the quartz tube. The CO flow rate is controlled at 20 mL / min, and the H2 flow rate is controlled at 30 mL / min. When the internal pressure of the quartz tube reaches 1 MPa, stop inputting CO and H. 2, Close the ventilation pipe valve;

[0089] Step 5: Heat to about 1240°C and maintain for 6 hours to allow the gallium and arsenic in the quartz tube to fully react to form a gallium arsenide solution; by controlling the vertical gradient condensation method, the temperature is controlled at 1238°C to move the gallium arsenide solid-liquid interface vertically upward from the bottom of the polycrystal. After 16 hours of gradient condensation, the condensation rate is controlled at 25mm / h to synthesize a hollow cylindrical carbon-doped gallium arsenide polycrystal with a diameter of 76mm and a length of 400mm. The overall average carbon concentration of the carbon-doped gallium arsenide polycrystal is 0.8×10 15 atoms / cm 3 .

[0090] The carbon-doped gallium arsenide polycrystal is further prepared to obtain a gallium arsenide single crystal, and the specific operation is as follows:

[0091] Step 1, placing a gallium arsenide seed crystal in a boron nitride crucible, placing the synthesized gallium arsenide polycrystal in a 6-inch boron nitride crucible, and placing 50g of boron oxide at the bottom of the crucible;

[0092] Step 2: Place the crucible containing gallium arsenide polycrystals into a stepped quartz tube, heat and seal the quartz cap and the stepped quartz tube, and place the sealed quartz tube in a single crystal growth furnace.

[0093] Step 3: The temperature of the single crystal growth furnace is raised to 1242° C. and heating is continued for 24 hours to completely melt the gallium arsenide polycrystal.

[0094] Step 4, by controlling the temperature gradient, the temperature of the seed crystal area at the bottom of the crucible is raised to 1237°C, so that the gallium arsenide solid-liquid interface moves vertically upward from the seed crystal area, and the growth rate is controlled to be 1 mm / h. After 150 hours of growth time, a 6-inch gallium arsenide single crystal is obtained.

[0095] Example 2

[0096] Step 1: Place a hollow cylindrical quartz crucible with a diameter of 100 mm and a length of 450 mm in the lower part of the stepped quartz tube, and place a quartz crucible with a hollow cone with a diameter of 150 mm in the upper part of the stepped quartz tube;

[0097] Step 2: The quartz cap and the quartz tube are vertically welded together with hydroxide to make the quartz tube and the quartz cap sealed and connected;

[0098] Step 3: Pour 10 kg of liquid 7N gallium into the hollow cylindrical quartz crucible, and put 11 kg of 7N arsenic into the hollow quartz crucible, and then vacuum weld and seal the quartz cap feed port.

[0099] Step 4: Place the welded quartz tube into the polycrystalline synthesis furnace, and input CO and H2 from the gas pipe at the bottom of the quartz tube. The CO flow rate is controlled at 25mL / min, and the H2 flow rate is controlled at 25mL / min. When the internal pressure of the quartz tube reaches 1.1MPa, stop inputting CO and H. 2, Close the ventilation pipe valve;

[0100] Step 5: Heat to about 1240°C and maintain for 10 hours to allow the gallium and arsenic in the quartz tube to fully react to form a gallium arsenide solution; by controlling the vertical gradient condensation method, the temperature is controlled at 1238°C to move the gallium arsenide solid-liquid interface vertically upward from the bottom of the polycrystal. After 24 hours of gradient condensation, the condensation rate is controlled at 16.7mm / h to synthesize a hollow cylindrical carbon-doped gallium arsenide polycrystal with a diameter of 100mm and a length of 400mm. The overall average carbon concentration of the carbon-doped gallium arsenide polycrystal is 1×10 15 atoms / cm 3 .

[0101] The carbon-doped gallium arsenide polycrystal is further prepared to obtain a gallium arsenide single crystal, and the specific operation is the same as the process of preparing the single crystal in Example 1.

[0102] Example 3

[0103] Step 1: Place a hollow cylindrical quartz crucible with a diameter of 150 mm and a length of 450 mm in the lower part of the stepped quartz tube, and place a quartz crucible with a conical hollow part with a diameter of 200 mm in the upper part of the stepped quartz tube;

[0104] Step 2: The quartz cap and the quartz tube are vertically welded together with hydroxide to make the quartz tube and the quartz cap sealed and connected;

[0105] Step 3: Pour 10KG of liquid 7N gallium into the hollow cylindrical quartz crucible, and put 12KG of 7N arsenic into the hollow quartz crucible, and then vacuum weld and seal the quartz cap feed port. The increase in the arsenic-gallium ratio is because the diameter of the quartz tube changes, the space inside the tube increases, and more As is needed to form As vapor at high temperature to maintain the pressure balance in the tube;

[0106] Step 4: Place the welded quartz tube into the polycrystalline synthesis furnace, and input CO and H2 from the gas pipe at the bottom of the quartz tube. The CO flow rate is controlled at 30mL / min, and the H2 flow rate is controlled at 30mL / min. When the internal pressure of the quartz tube reaches 1.2MPa, stop inputting CO and H. 2, Close the ventilation pipe valve;

[0107] Step 5: Heat to about 1240°C and maintain for 10 hours to allow the gallium and arsenic in the quartz tube to fully react to form a gallium arsenide solution; by controlling the vertical gradient condensation method, the temperature is controlled at 1238°C to move the gallium arsenide solid-liquid interface vertically upward from the bottom of the polycrystal. After 24 hours of gradient condensation, the condensation rate is controlled at 8.33mm / h to synthesize a hollow cylindrical carbon-doped gallium arsenide polycrystal with a diameter of 150mm and a length of 200mm. The overall average carbon concentration of the carbon-doped gallium arsenide polycrystal is 1.1×10 15 atoms / cm 3 .

[0108] The carbon-doped gallium arsenide polycrystal is further prepared to obtain a gallium arsenide single crystal, and the specific operation is the same as the process of preparing the single crystal in Example 1.

[0109] Example 4

[0110] The embodiment of the present invention provides a gallium arsenide polycrystal and a synthesis method. The only difference between the gallium arsenide polycrystal and the synthesis method and the embodiment 2 is that in step (4), the CO flow rate is controlled at 30 mL / min. A hollow cylindrical carbon-doped gallium arsenide polycrystal with a diameter of 100 mm and a length of 450 mm is synthesized. The overall average carbon concentration of the carbon-doped gallium arsenide polycrystal is 1.2×10 15 atoms / cm 3 .

[0111] The carbon-doped gallium arsenide polycrystal is further prepared to obtain a gallium arsenide single crystal, and the specific operation is the same as the process of preparing the single crystal in Example 1.

[0112] Comparative Example 1

[0113] The traditional method for synthesizing gallium arsenide polycrystals is to use the horizontal Bridgman synthesis method;

[0114] Step 1: Put 3KG of 7N gallium and 3.3KG of 7N arsenic into 3-inch boat-shaped boron nitride crucibles respectively;

[0115] Step 2: Place the crucible filled with gallium and arsenic horizontally into the quartz tube, put a quartz cap into the mouth of the quartz tube, and then vacuum weld the quartz cap and the quartz tube to make it vacuum-tight;

[0116] Step 3: Place the sealed quartz tube horizontally into the polycrystalline synthesis furnace, adjust the temperature gradient, and synthesize a D-shaped gallium arsenide polycrystalline material with a diameter of 76 mm, a height of 70 mm, and a length of 300 mm; The gallium arsenide polycrystalline materials prepared in the above Examples 1 to 4 and Comparative Example 1 are subjected to performance tests, and the test results are shown in Table 1.

[0117] Table 1 Size and performance test of polycrystals prepared in Examples 1 to 4 and Comparative Example 1 and the dislocation density and electrical performance uniformity results of single crystals grown from the polycrystals

[0118] Table 1 Performance test results

[0119]

[0120]

[0121] By comparing Examples 1 to 4 with Comparative Example 1, each furnace of polycrystalline material and the semi-insulating gallium arsenide single crystal grown using the polycrystalline material were tested for Hall (Hall effect) and EPD (dislocation density) at the head and tail positions, and 5 points were taken at the head and tail respectively, and then the 5 points were averaged and the 5-point average was used as the uniformity data result for comparison. Among them, since gallium arsenide polycrystalline and single crystal are grown from bottom to top in the above-mentioned device, the grown single crystal or polycrystalline is the head and tail from bottom to top.

[0122] The Hall test is to take a wafer from the head and tail of the wafer, and then take a point in the middle and four sides of the wafer to test the Hall, and obtain the interception carrier concentration data and resistivity. EPD detection is to use automatic detection equipment to scan the entire wafer to read the EPD (dislocation density) number. Due to the crystal segregation effect, dopants and impurities flow faster into the liquid than the solid, so the carrier concentration and resistance of the tail of the carbon-doped gallium arsenide polycrystalline crystal are higher than those of the head, and because the impurities in the tail are more concentrated, its uniformity is worse than that of the head. Similarly, due to the crystal segregation effect, the dislocation density of the tail of the semi-insulating gallium arsenide single crystal is higher than that of the head.

[0123] By comparing Example 1, Example 2 and Example 3, the results show that when preparing the carbon-doped gallium arsenide polycrystal of the present invention, the greater the condensation rate, the greater the resistance change of the polycrystal, the lower the uniformity of the electrical properties of the semi-insulating gallium arsenide single crystal prepared using the polycrystal, and the dislocation density also shows an increasing trend.

[0124] Comparing Example 2 and Example 4, the results show that increasing the flow rate of CO will increase the head-to-tail resistivity, but the corresponding uniformity will deteriorate, because increasing CO increases the concentration of the dopant C, and the C element is a factor that affects the resistivity. The higher the C content of the gallium arsenide polycrystalline material, the higher the resistivity. In addition, when H2 decreases, its reaction with metal impurities decreases, that is, the metal impurities become more and are distributed in the polycrystalline, affecting the uniformity of the electrical properties of the gallium arsenide polycrystalline. By adding CO and H2, Examples 1 to 4 make the carrier concentration and resistivity of the prepared carbon-doped gallium arsenide polycrystalline material change greatly, the resistivity increases by nearly 10 orders of magnitude, and the carrier concentration decreases by nearly 10 orders of magnitude. Moreover, the carbon-doped gallium arsenide polycrystalline material synthesized by the present invention is a hollow cylindrical shape, while the gallium arsenide polycrystalline material prepared in Comparative Example 1 is D-shaped. The weight of a tube of polycrystalline (i.e., gallium arsenide polycrystalline under one experimental operation) synthesized in any of Examples 1 to 4 is increased by more than 100% compared with Comparative Example 1.

[0125] By comparing the results of Examples 1 to 4 with Comparative Example 1, it is shown that the semi-insulating gallium arsenide single crystal prepared by using the carbon-doped gallium arsenide polycrystal of the present invention as the raw material of the gallium arsenide single crystal has the advantages of more uniform electrical property distribution and lower dislocation density. The description of the above embodiments is only used to help understand the method of the present invention and its core idea. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, several improvements and modifications can be made to the present invention, and these improvements and modifications also fall within the scope of protection of the claims of the present invention.

Claims

1. A carbon-doped gallium arsenide polycrystal, characterized in that: Its carbon concentration is (0.2~2)×10 15 atoms / cm 3 ; The carbon-doped gallium arsenide polycrystal has a hollow cylindrical structure; The outer diameter of the hollow cylindrical structure is 76 to 150 mm, and the inner diameter is 10 to 20 mm; The height of the hollow cylindrical structure is 200-400 mm.

2. The carbon-doped gallium arsenide polycrystal according to claim 1, characterized in that: The sum of other impurities in the carbon-doped gallium arsenide polycrystal is less than 100 PPB.

3. The carbon-doped gallium arsenide polycrystal according to claim 1 or 2, characterized in that: The carrier concentration of the carbon-doped gallium arsenide polycrystal is (1-60)×10 6 cm 3 ; The resistivity of the carbon-doped gallium arsenide polycrystal is (1-10)×10 8 ohm.cm.

4. A device for preparing the carbon-doped gallium arsenide polycrystal according to any one of claims 1 to 3, characterized in that: It comprises a polycrystal synthesis furnace and a stepped quartz tube arranged inside the polycrystal synthesis furnace; The stepped quartz tube comprises a tube body, one end of which is open, and the other end of which is provided with a Y-shaped gas delivery pipe for delivering hydrogen and carbon monoxide; The tube body comprises two coaxially arranged tube body units, the tube body units are in the shape of a circular tube, and the diameters of the two tube body units gradually increase from the Y-shaped gas delivery pipe to the opening; The upper tube unit of the stepped quartz tube is provided with a quartz crucible with a hollow cone, and the lower tube unit is provided with a hollow cylindrical quartz crucible. The upper tube unit is the tube unit in the opening direction. The hollow cylindrical quartz crucible comprises a quartz crucible with a conical bottom and a hollow cylinder arranged inside the crucible; The top of the hollow cylinder is sealed and small holes are provided on both sides for the introduction of gas; A quartz cap is provided on the top of the stepped quartz tube; The top of the quartz cap is provided with a feed port for feeding or vacuuming; the Y-shaped gas pipe is provided with a ventilation pipe valve for controlling the flow of the incoming gas.

5. The device according to claim 4, characterized in that The outer diameter of the hollow cylindrical quartz crucible is 76-150 mm, and the inner diameter is 10-20 mm; The length of the hollow cylindrical quartz crucible is 200-450 mm.

6. The device according to claim 4, characterized in that The diameter of the quartz crucible with a hollow cone portion is 1.2 to 1.5 times the outer diameter of the hollow cylindrical quartz crucible.

7. A method for preparing carbon-doped gallium arsenide polycrystal, characterized in that: The method is carried out using the device according to any one of claims 4 to 6, comprising the following steps: 1) placing liquid 7N gallium and solid 7N arsenic in a hollow cylindrical quartz crucible and a quartz crucible with a hollow cone, respectively, and then evacuating to maintain a sealed vacuum environment of the stepped quartz tube; 2) placing the stepped quartz tube in a polycrystalline synthesis furnace, and simultaneously introducing carbon monoxide and hydrogen from the Y-shaped gas pipe of the device into the liquid 7N gallium, so that the pressure inside the stepped quartz tube is 1-1.5 MPa, and then heating until the solid 7N arsenic is vaporized, and the vaporized 7N arsenic is mixed with the liquid gallium to react, so as to obtain a gallium arsenide solution; 3) The gallium arsenide solution is subjected to a vertical gradient condensation method to prepare the carbon-doped gallium arsenide polycrystal.

8. The preparation method according to claim 7, characterized in that: The specific conditions of the vertical gradient condensation method in step 4) are: The temperature is 1235℃~1245℃; Gradient condensation time is 16 to 24 h; The condensation rate is 8-25 mm / h.

9. The preparation method according to claim 7, characterized in that: The heating temperature in step 3) is 1240°C to 1250°C; The heating time is 6 to 10 hours; In the step 1), the mass ratio of solid 7N arsenic to liquid 7N gallium is (1.1-1.2):1; The flow rate of carbon monoxide in step 2) is 20-30 mL / min; The flow rate of hydrogen in the step 2) is 20-30 mL / min.

10. A gallium arsenide single crystal, characterized in that: The method is prepared by using the carbon-doped gallium arsenide polycrystal according to any one of claims 1 to 3 or the carbon-doped gallium arsenide polycrystal prepared by the preparation method according to any one of claims 7 to 9.