Flame-retardant composite colored spun yarn and preparation method thereof
The reaction of the modified filler and monomer is to form a spinning liquid, imidized and dyed at high temperatures, and form a multi-layer carbon layer, which solves the problem of poor flame retardant effect of color spinning and significantly improves its flame retardant performance.
Patent Information
- Application Number
- CN202411048513.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-08-01
AI Technical Summary
At this stage, the flame retardant effect of color spinning is poor, resulting in dripping and smoldering during the combustion process, narrowing its scope of use.
Using a mixture of modified filler, 3-isocyanate propylmethyldimethoxysilane and toluene, combined with 3,3',4,4'-biphenyltetracarboxylic dianhydride, p-phenylenediamine and modified monomer , the spinning liquid is formed by stirring and reaction, and then imidized under high temperature conditions to form reinforced fibers, dyeing and multi-layer carbon layers to improve flame retardant performance.
Through internal organophosphorus, phosphoric anhydride and phosphides form a carbonized layer, combined with doping of silicon, nitrogen and boron elements, a dense carbon layer is formed, which significantly improves the flame retardant effect and reduces the generation of toxic flue gas, significantly improving the color spinning Flame retardant performance.
Smart Images

Figure BDA0004974196760000141
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of colored spun yarn preparation, and in particular to a flame-retardant composite colored spun yarn and a preparation method thereof. Background Art
[0002] Colored yarn is to dye the fiber into colored fiber first, and then mix two or more fibers of different colors fully to spin into yarn with unique color mixing effect. Human beings have a long history of using fiber materials. From natural fibers such as cotton, linen, silk, wool to synthetic fibers such as nylon, acrylic, Teflon, etc., they have always been important thermal insulation materials for humans. Although synthetic fiber materials were born relatively late, their high performance, high strength, high precision and other characteristics are not possessed by natural fiber materials. Therefore, most fabrics on the market today are composite fabrics made of synthetic fibers. However, synthetic fibers have poor flame retardancy. During the combustion process, they will drip and even smolder, resulting in secondary combustion, which reduces the scope of use of colored yarn. Summary of the invention
[0003] The purpose of the present invention is to provide a flame retardant composite color spun yarn and a preparation method thereof, so as to solve the problem that the flame retardant effect of the color spun yarn is not good at the current stage.
[0004] The purpose of the present invention can be achieved through the following technical solutions:
[0005] A method for preparing a flame-retardant composite colored spun yarn comprises the following steps:
[0006] Step S1: mixing the modified filler, 3-isocyanatepropylmethyldimethoxysilane and toluene, stirring for 3-5 hours at a speed of 120-150 r / min and a temperature of 25-30° C. to obtain a functional filler, uniformly mixing 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, the modified monomer and N,N-dimethylacetamide, stirring for 3-5 hours at a speed of 120-150 r / min and a temperature of 40-45° C., cooling to 0° C., stirring for 40-45 hours, adding the functional filler, stirring for 3-5 hours, and obtaining a spinning solution;
[0007] Step S2: The spinning solution is squeezed into a coagulation bath through a spinneret with 100 holes and a diameter of 75 microns under a nitrogen pressure of 0.3-0.35 MPa, and then kept warm for 1 hour at 100°C, 280°C and 350°C respectively to obtain reinforced fibers, and the reinforced fibers are dyed to obtain dyed fibers, and the dyed fibers are opened, carded, drawn, roving and spinning to obtain pretreated yarns, and the pretreated yarns are immersed in deionized water, kept warm for 3-5 hours at a temperature of 60-70°C, taken out and dried to obtain flame-retardant composite color spun yarns.
[0008] Furthermore, the amount ratio of the modified filler and 3-isocyanatepropylmethyldimethoxysilane described in step S1 is 1g:3mL, and the amount ratio of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, modified monomer, N,N-dimethylacetamide and functional filler is 55mmo l:40mmol:15mmo l:60mL:5g.
[0009] Further, the modified monomer is prepared by the following steps:
[0010] Step A1: Phosphorus oxychloride, 2,2-dihydroxymethylpropionic acid and N,N-dimethylformamide are uniformly mixed, and reacted for 6-8 hours at a speed of 120-150 r / min and a temperature of 100-110° C. to obtain intermediate 1; intermediate 1 is dissolved in N,N-dimethylformamide, nitrogen is introduced for protection, and formic acid is added under stirring at a speed of 150-200 r / min and a temperature of 30-40° C. to react for 4-6 hours to obtain a phosphorus additive; the phosphorus additive, KH550, dicyclohexylcarbodiimide and N,N-dimethylformamide are mixed, and reacted for 3-5 hours at a speed of 120-150 r / min and a temperature of 30-40° C. to obtain a phosphorus modifier;
[0011] Step A2: octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed uniformly, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 120-150 r / min and a temperature of 90-100° C. to obtain a diamine-terminated polysiloxane; the diamine-terminated polysiloxane, a phosphorus modifier and N,N-dimethylformamide are mixed uniformly, nitrogen is introduced for protection, and the reaction is carried out for 40-45 hours at a speed of 150-200 r / min and a temperature of 65-70° C. to obtain a modified monomer.
[0012] Furthermore, the molar ratio of phosphorus oxychloride and 2,2-dihydroxymethylpropionic acid in step A1 is 1:1, the molar ratio of intermediate 1 and formic acid is 1:1, and the molar ratio of phosphorus additive, KH550 and dicyclohexylcarbodiimide is 1:1:1.1.
[0013] Furthermore, the molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A2 is 1.8:0.6:2:3, and the molar ratio of the double bond on the diamine-terminated polysiloxane and the phosphorus modifier is 1:1.
[0014] Further, the modified filler is prepared by the following steps:
[0015] Step B1: melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and methanol are mixed, stirred and hydrochloric acid solution is added at a speed of 120-150 r / min and a temperature of 20-25° C., and the temperature is raised to 65-70° C. to react for 3-5 hours to obtain intermediate 2; 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and N,N-dimethylformamide are mixed uniformly, and the reaction is carried out at a speed of 150-200 r / min and a temperature of 60-70° C. for 2-4 hours, and then sodium hydroxide solution is added, the temperature is raised to 80-85° C., and the reaction is carried out for 4-6 hours to obtain intermediate 3;
[0016] Step B2: Mix intermediate 3, sodium periodate, tetrahydrofuran and deionized water uniformly, stir and add hydrochloric acid solution at a speed of 120-150 r / min and a temperature of 25-30°C, and react for 3-4 hours to obtain intermediate 4; mix intermediate 2, intermediate 4, 5A molecular sieve and N,N-dimethylformamide uniformly, and react for 10-15 hours at a speed of 120-150 r / min and a temperature of 60-70°C to obtain intermediate 5;
[0017] Step B3: The intermediate 5, 2-aminoterephthalic acid and N,N-dimethylformamide are mixed, and the reaction is carried out for 4-6 hours at a speed of 150-200 r / min, a temperature of 20-25°C, and a pH value of 11-12. The pH is adjusted to be acidic, the temperature is raised to 85-90°C, DOPO is added, and the reaction is continued for 6-8 hours to obtain an organic ligand. The organic ligand, samarium nitrate hexahydrate and N,N-dimethylformamide are mixed uniformly, and deionized water is added at a speed of 120-150 r / min and a temperature of 20-25°C. After stirring for 20-30 minutes, the temperature is raised to 105-110°C, and the reaction is carried out for 10-15 hours to obtain a modified filler.
[0018] Further, the amount ratio of melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and hydrochloric acid solution in step B1 is 50mmo l:150mmo l:1g:2mL, the mass fraction of hydrochloric acid solution is 10%, the amount ratio of 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 10mmo l:10mmo l:0.5g:30mL, and the mass fraction of sodium hydroxide solution is 10%.
[0019] Furthermore, the amount ratio of intermediate 3, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 5mmo l:15mmo l:40mL:10mL:3.5mL, the mass fraction of hydrochloric acid solution is 5%, and the amount ratio of intermediate 2, intermediate 4 and 5A molecular sieve is 10mmo l:30mmo l:2g.
[0020] Furthermore, the molar ratio of the intermediate 5, 2-aminoterephthalic acid and DOPO described in step B3 is 1:3:3, and the dosage ratio of the organic ligand, samarium nitrate hexahydrate, N,N-dimethylformamide and deionized water is 1.5 mmol:1 mmol:50 mL:5 mL.
[0021] Beneficial effects of the present invention: A flame-retardant composite colored spun yarn prepared by the present invention is formed by reacting 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine and a modified monomer to form polyamic acid, which is then blended with a functional filler to obtain a spinning solution, which is spun and imidized under high temperature conditions to obtain a reinforced fiber, which is dyed to obtain a dyed fiber, which is subjected to opening, carding, drawing, roving and spinning processes to obtain a pretreated yarn, which is immersed in a ferric chloride solution, taken out and dried to obtain a colored spun yarn, and the modified monomer is reacted with phosphorus oxychloride and 2,2-dimethylolpropionic acid so that the chlorine atom site on the phosphorus oxychloride reacts with the hydroxyl group on the 2,2-dimethylolpropionic acid. , obtain intermediate 1, treat intermediate 1 with formic acid to convert the P-Cl bond on intermediate 1 into a PH bond to obtain a phosphorus additive, react the phosphorus additive with KH550 to react the carboxyl group on the phosphorus additive with the amino group on KH550 to obtain a phosphorus modifier, ring-open octamethylcyclotetrasiloxane and 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, and then polymerize with 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane to form a diamine-terminated polysiloxane, react the diamine-terminated polysiloxane with a phosphorus modifier to react the double bond on the diamine-terminated polysiloxane with the PH bond on the phosphorus modifier to obtain a modified monomer.
[0022] The functional filler uses melamine and 3,4-dihydroxybenzaldehyde as raw materials, so that the amino group on the melamine reacts with the aldehyde group on the 3,4-dihydroxybenzaldehyde to obtain intermediate 2, 4-hydroxyphenylboronic acid pinacol ester reacts with epichlorohydrin, so that the phenolic hydroxyl group on the 4-hydroxyphenylboronic acid pinacol ester reacts with the epoxy group on the epichlorohydrin, and then the ring is closed under the action of sodium hydroxide solution to form a new epoxy group to obtain intermediate 3, and intermediate 3 is treated with sodium periodate to convert the structure of phenylboronic acid pinacol ester into a phenylboronic acid structure to obtain intermediate 4, and intermediate 4 and intermediate 2 are reacted. The invention relates to a method for preparing a functional filler by reacting the intermediate 4 with the catechol structure on the intermediate 2, wherein the phenylboric acid on the intermediate 4 reacts with the catechol structure on the intermediate 2 to obtain the intermediate 5; the intermediate 5 reacts with 2-aminoterephthalic acid to react the epoxy group on the intermediate 5 with the amino group on the 2-aminoterephthalic acid to obtain the organic ligand; the organic ligand reacts with samarium nitrate hexahydrate to form an organic framework of samarium to obtain the modified filler; the modified filler is treated with 3-isocyanatepropylmethyldimethoxysilane to react the hydroxyl group on the surface of the modified filler with the isocyanate group on the 3-isocyanatepropylmethyldimethoxysilane to obtain the functional filler.
[0023] When the colored yarn burns, the organic phosphorus inside can generate phosphoric anhydride and phosphide. Phosphoric anhydride can dehydrate and carbonize the colored yarn, forming a carbonized layer on the surface to isolate the external heat. At the same time, it contains silicon, nitrogen and boron elements, which further improves the density of the carbon layer and can release nitrogen and nitrogen dioxide gases, thereby reducing the oxygen content and improving the flame retardant effect. The organic framework containing the rare earth metal samarium can reduce the generation of toxic smoke. When the pretreated yarn is immersed in deionized water, the siloxane on the side chain of the polyimide molecule and the siloxane on the surface of the functionalized filler can hydrolyze and condense, and then during the carbonization process, a multi-layer carbon layer is formed, which further improves the flame retardant effect. DETAILED DESCRIPTION
[0024] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] Example 1
[0026] A method for preparing a flame-retardant composite colored spun yarn comprises the following steps:
[0027] Step S1: Mix the modified filler, 3-isocyanatepropylmethyldimethoxysilane and toluene, stir for 3 hours at a speed of 120 r / min and a temperature of 25° C. to obtain a functional filler, mix 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, the modified monomer and N,N-dimethylacetamide evenly, stir for 3 hours at a speed of 120 r / min and a temperature of 40° C., cool to 0° C., stir for 40 hours, add the functional filler, stir for 3 hours, and obtain a spinning solution;
[0028] Step S2: The spinning solution is squeezed into a coagulation bath through a spinneret with 100 holes and a diameter of 75 microns under a nitrogen pressure of 0.3 MPa, and then kept warm for 1 hour at 100°C, 280°C and 350°C respectively to obtain reinforced fibers, and the reinforced fibers are dyed to obtain dyed fibers, and the dyed fibers are subjected to opening, carding, drawing, roving and spinning processes to obtain pretreated yarns, and the pretreated yarns are immersed in deionized water, kept warm for 3 hours at 60°C, taken out and dried to obtain flame-retardant composite color spun yarns.
[0029] The amount ratio of the modified filler and 3-isocyanatepropylmethyldimethoxysilane described in step S1 is 1g:3mL, and the amount ratio of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, modified monomer, N,N-dimethylacetamide and functional filler is 55mmo l:40mmo l:15mmo l:60mL:5g.
[0030] The modified monomer is prepared by the following steps:
[0031] Step A1: Phosphorus oxychloride, 2,2-dihydroxymethylpropionic acid and N,N-dimethylformamide are uniformly mixed, and reacted for 6 hours at a speed of 120 r / min and a temperature of 100° C. to obtain intermediate 1; intermediate 1 is dissolved in N,N-dimethylformamide, nitrogen is introduced for protection, and formic acid is added under stirring at a speed of 150 r / min and a temperature of 30° C. to react for 4 hours to obtain a phosphorus additive; the phosphorus additive, KH550, dicyclohexylcarbodiimide and N,N-dimethylformamide are mixed, and reacted for 3 hours at a speed of 120 r / min and a temperature of 30° C. to obtain a phosphorus modifier;
[0032] Step A2: octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 3 hours at a speed of 120 r / min and a temperature of 90° C. to obtain a diamine-terminated polysiloxane; the diamine-terminated polysiloxane, a phosphorus modifier and N,N-dimethylformamide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 40 hours at a speed of 150 r / min and a temperature of 65° C. to obtain a modified monomer.
[0033] The molar ratio of phosphorus oxychloride and 2,2-dihydroxymethylpropionic acid in step A1 is 1:1, the molar ratio of intermediate 1 and formic acid is 1:1, and the molar ratio of phosphorus additive, KH550 and dicyclohexylcarbodiimide is 1:1:1.1.
[0034] The molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A2 is 1.8:0.6:2:3, and the molar ratio of the double bond on the diamine-terminated polysiloxane and the phosphorus modifier is 1:1.
[0035] The modified filler is prepared by the following steps:
[0036] Step B1: melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and methanol are mixed, stirred and hydrochloric acid solution is added at a speed of 120 r / min and a temperature of 20°C, and the temperature is raised to 65°C for reaction for 3 hours to obtain intermediate 2; 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and N,N-dimethylformamide are mixed evenly, reacted at a speed of 150 r / min and a temperature of 60°C for 2 hours, and then sodium hydroxide solution is added, the temperature is raised to 80°C, and the reaction is carried out for 4 hours to obtain intermediate 3;
[0037] Step B2: Intermediate 3, sodium periodate, tetrahydrofuran and deionized water were mixed evenly, stirred and hydrochloric acid solution was added at a speed of 120 r / min and a temperature of 25°C, and reacted for 3 hours to obtain intermediate 4; intermediate 2, intermediate 4, 5A molecular sieve and N,N-dimethylformamide were mixed evenly, and reacted at a speed of 120 r / min and a temperature of 60°C for 10 hours to obtain intermediate 5;
[0038] Step B3: The intermediate 5, 2-aminoterephthalic acid and N,N-dimethylformamide are mixed, and the reaction is carried out for 4 hours at a speed of 150 r / min, a temperature of 20°C and a pH value of 11, and the pH is adjusted to be acidic, the temperature is raised to 85°C, DOPO is added, and the reaction is continued for 6 hours to obtain an organic ligand. The organic ligand, samarium nitrate hexahydrate and N,N-dimethylformamide are mixed evenly, and deionized water is added at a speed of 120 r / min and a temperature of 20°C. After stirring for 20 minutes, the temperature is raised to 105°C and the reaction is carried out for 10 hours to obtain a modified filler.
[0039] The amount ratio of melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and hydrochloric acid solution described in step B1 is 50mmo l:150mmo l:1g:2mL, the mass fraction of hydrochloric acid solution is 10%, the amount ratio of 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 10mmo l:10mmo l:0.5g:30mL, and the mass fraction of sodium hydroxide solution is 10%.
[0040] The amount ratio of intermediate 3, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 5mmo l:15mmo l:40mL:10mL:3.5mL, the mass fraction of hydrochloric acid solution is 5%, and the amount ratio of intermediate 2, intermediate 4 and 5A molecular sieve is 10mmo l:30mmo l:2g.
[0041] The molar ratio of the intermediate 5, 2-aminoterephthalic acid and DOPO described in step B3 is 1:3:3, and the amount ratio of the organic ligand, samarium nitrate hexahydrate, N,N-dimethylformamide and deionized water is 1.5 mmol:1 mmol:50 mL:5 mL.
[0042] Example 2
[0043] A method for preparing a flame-retardant composite colored spun yarn comprises the following steps:
[0044] Step S1: Mix the modified filler, 3-isocyanatepropylmethyldimethoxysilane and toluene, stir for 4 hours at a speed of 120-150 r / min and a temperature of 25°C to obtain a functional filler, mix 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, the modified monomer and N,N-dimethylacetamide evenly, stir for 4 hours at a speed of 150 r / min and a temperature of 40°C, cool to 0°C, stir for 45 hours, add the functional filler, stir for 4 hours, and obtain a spinning solution;
[0045] Step S2: The spinning solution is squeezed into a coagulation bath through a spinneret with 100 holes and a diameter of 75 microns under a nitrogen pressure of 0.3 MPa, and then kept warm for 1 hour at 100°C, 280°C and 350°C to obtain reinforced fibers. The reinforced fibers are dyed to obtain dyed fibers. The dyed fibers are opened, carded, drawn, roving and spinning to obtain pretreated yarns. The pretreated yarns are immersed in deionized water, kept warm for 4 hours at 65°C, taken out and dried to obtain flame-retardant composite color spun yarns.
[0046] The amount ratio of the modified filler and 3-isocyanatepropylmethyldimethoxysilane described in step S1 is 1g:3mL, and the amount ratio of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, modified monomer, N,N-dimethylacetamide and functional filler is 55mmo l:40mmo l:15mmo l:60mL:5g.
[0047] The modified monomer is prepared by the following steps:
[0048] Step A1: Phosphorus oxychloride, 2,2-dihydroxymethylpropionic acid and N,N-dimethylformamide are uniformly mixed, and reacted for 7 hours at a speed of 120 r / min and a temperature of 105° C. to obtain intermediate 1; intermediate 1 is dissolved in N,N-dimethylformamide, nitrogen is introduced for protection, and formic acid is added under stirring at a speed of 150 r / min and a temperature of 35° C. to react for 5 hours to obtain a phosphorus additive; the phosphorus additive, KH550, dicyclohexylcarbodiimide and N,N-dimethylformamide are mixed, and reacted for 4 hours at a speed of 120 r / min and a temperature of 35° C. to obtain a phosphorus modifier;
[0049] Step A2: octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 4 hours at a speed of 150 r / min and a temperature of 95° C. to obtain a diamine-terminated polysiloxane; the diamine-terminated polysiloxane, a phosphorus modifier and N,N-dimethylformamide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 45 hours at a speed of 150 r / min and a temperature of 65° C. to obtain a modified monomer.
[0050] The molar ratio of phosphorus oxychloride and 2,2-dihydroxymethylpropionic acid in step A1 is 1:1, the molar ratio of intermediate 1 and formic acid is 1:1, and the molar ratio of phosphorus additive, KH550 and dicyclohexylcarbodiimide is 1:1:1.1.
[0051] The molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A2 is 1.8:0.6:2:3, and the molar ratio of the double bond on the diamine-terminated polysiloxane and the phosphorus modifier is 1:1.
[0052] The modified filler is prepared by the following steps:
[0053] Step B1: melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and methanol are mixed, stirred and hydrochloric acid solution is added at a speed of 120 r / min and a temperature of 25°C, and the temperature is raised to 65°C for reaction for 4 hours to obtain intermediate 2; 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and N,N-dimethylformamide are mixed evenly, reacted at a speed of 150 r / min and a temperature of 65°C for 3 hours, and then sodium hydroxide solution is added, the temperature is raised to 80°C, and the reaction is carried out for 5 hours to obtain intermediate 3;
[0054] Step B2: Intermediate 3, sodium periodate, tetrahydrofuran and deionized water were mixed evenly, stirred and hydrochloric acid solution was added at a speed of 150 r / min and a temperature of 25°C, and reacted for 5 hours to obtain intermediate 4; intermediate 2, intermediate 4, 5A molecular sieve and N,N-dimethylformamide were mixed evenly, and reacted at a speed of 120 r / min and a temperature of 65°C for 15 hours to obtain intermediate 5;
[0055] Step B3: The intermediate 5, 2-aminoterephthalic acid and N,N-dimethylformamide are mixed, and the reaction is carried out for 5 hours at a speed of 200 r / min, a temperature of 20°C and a pH value of 11, and the pH is adjusted to be acidic, the temperature is raised to 85°C, DOPO is added, and the reaction is continued for 7 hours to obtain an organic ligand. The organic ligand, samarium nitrate hexahydrate and N,N-dimethylformamide are mixed evenly, and deionized water is added at a speed of 150 r / min and a temperature of 20°C. After stirring for 25 minutes, the temperature is raised to 110°C and the reaction is carried out for 10 hours to obtain a modified filler.
[0056] The amount ratio of melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and hydrochloric acid solution described in step B1 is 50mmo l:150mmo l:1g:2mL, the mass fraction of hydrochloric acid solution is 10%, the amount ratio of 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 10mmo l:10mmo l:0.5g:30mL, and the mass fraction of sodium hydroxide solution is 10%.
[0057] The amount ratio of intermediate 3, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 5mmo l:15mmo l:40mL:10mL:3.5mL, the mass fraction of hydrochloric acid solution is 5%, and the amount ratio of intermediate 2, intermediate 4 and 5A molecular sieve is 10mmo l:30mmo l:2g.
[0058] The molar ratio of the intermediate 5, 2-aminoterephthalic acid and DOPO described in step B3 is 1:3:3, and the amount ratio of the organic ligand, samarium nitrate hexahydrate, N,N-dimethylformamide and deionized water is 1.5 mmol:1 mmol:50 mL:5 mL.
[0059] Example 3
[0060] A method for preparing a flame-retardant composite colored spun yarn comprises the following steps:
[0061] Step S1: Mix the modified filler, 3-isocyanatepropylmethyldimethoxysilane and toluene, stir for 5 hours at a speed of 150 r / min and a temperature of 30° C. to obtain a functional filler, mix 3,3',4,4'-biphenyltetracarboxylic acid anhydride, p-phenylenediamine, the modified monomer and N,N-dimethylacetamide evenly, stir for hours at a speed of 150 r / min and a temperature of 45° C., cool to 0° C., stir for 45 hours, add the functional filler, stir for 5 hours, and obtain a spinning solution;
[0062] Step S2: The spinning solution is squeezed into a coagulation bath through a spinneret with 100 holes and a diameter of 75 microns under a nitrogen pressure of 0.35 MPa, and then kept warm for 1 hour at 100°C, 280°C and 350°C to obtain reinforced fibers. The reinforced fibers are dyed to obtain dyed fibers. The dyed fibers are opened, carded, drawn, roving and spinning to obtain pretreated yarns. The pretreated yarns are immersed in deionized water, kept warm for 5 hours at 70°C, taken out and dried to obtain flame-retardant composite color spun yarns.
[0063] The amount ratio of the modified filler and 3-isocyanatepropylmethyldimethoxysilane described in step S1 is 1g:3mL, and the amount ratio of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, modified monomer, N,N-dimethylacetamide and functional filler is 55mmo l:40mmo l:15mmo l:60mL:5g.
[0064] The modified monomer is prepared by the following steps:
[0065] Step A1: Phosphorus oxychloride, 2,2-dihydroxymethylpropionic acid and N,N-dimethylformamide are uniformly mixed, and reacted at a speed of 150 r / min and a temperature of 110° C. for 8 hours to obtain intermediate 1; intermediate 1 is dissolved in N,N-dimethylformamide, nitrogen is introduced for protection, and formic acid is added under stirring at a speed of 200 r / min and a temperature of 40° C., and the reaction is carried out for 6 hours to obtain a phosphorus additive; the phosphorus additive, KH550, dicyclohexylcarbodiimide and N,N-dimethylformamide are mixed, and reacted at a speed of 150 r / min and a temperature of 40° C. for 5 hours to obtain a phosphorus modifier;
[0066] Step A2: octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 5 hours at a speed of 150 r / min and a temperature of 100° C. to obtain a diamine-terminated polysiloxane; the diamine-terminated polysiloxane, a phosphorus modifier and N,N-dimethylformamide are mixed evenly, nitrogen is introduced for protection, and the reaction is carried out for 45 hours at a speed of 200 r / min and a temperature of 70° C. to obtain a modified monomer.
[0067] The molar ratio of phosphorus oxychloride and 2,2-dihydroxymethylpropionic acid in step A1 is 1:1, the molar ratio of intermediate 1 and formic acid is 1:1, and the molar ratio of phosphorus additive, KH550 and dicyclohexylcarbodiimide is 1:1:1.1.
[0068] The molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A2 is 1.8:0.6:2:3, and the molar ratio of the double bond on the diamine-terminated polysiloxane and the phosphorus modifier is 1:1.
[0069] The modified filler is prepared by the following steps:
[0070] Step B1: melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and methanol are mixed, stirred and hydrochloric acid solution is added at a speed of 150 r / min and a temperature of 25°C, and the temperature is raised to 70°C for reaction for 5 hours to obtain intermediate 2; 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and N,N-dimethylformamide are mixed uniformly, and the speed is 200 r / min and the temperature is 70°C for reaction for 4 hours, and then sodium hydroxide solution is added, the temperature is raised to 85°C, and the reaction is carried out for 6 hours to obtain intermediate 3;
[0071] Step B2: Intermediate 3, sodium periodate, tetrahydrofuran and deionized water were mixed evenly, stirred and hydrochloric acid solution was added at a speed of 150 r / min and a temperature of 30°C, and the reaction was carried out for 4 hours to obtain intermediate 4; intermediate 2, intermediate 4, 5A molecular sieve and N,N-dimethylformamide were mixed evenly, and the reaction was carried out at a speed of 150 r / min and a temperature of 70°C for 15 hours to obtain intermediate 5;
[0072] Step B3: The intermediate 5, 2-aminoterephthalic acid and N,N-dimethylformamide are mixed, and the reaction is carried out for 6 hours at a speed of 200 r / min, a temperature of 25°C and a pH value of 12. Then, the pH is adjusted to be acidic, the temperature is raised to 90°C, DOPO is added, and the reaction is continued for 8 hours to obtain an organic ligand. The organic ligand, samarium nitrate hexahydrate and N,N-dimethylformamide are mixed evenly, and deionized water is added at a speed of 150 r / min and a temperature of 25°C. After stirring for 30 minutes, the temperature is raised to 110°C and the reaction is carried out for 15 hours to obtain a modified filler.
[0073] The amount ratio of melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and hydrochloric acid solution described in step B1 is 50mmo l:150mmo l:1g:2mL, the mass fraction of hydrochloric acid solution is 10%, the amount ratio of 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and sodium hydroxide solution is 10mmo l:10mmo l:0.5g:30mL, and the mass fraction of sodium hydroxide solution is 10%.
[0074] The amount ratio of intermediate 3, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution described in step B2 is 5mmo l:15mmo l:40mL:10mL:3.5mL, the mass fraction of hydrochloric acid solution is 5%, and the amount ratio of intermediate 2, intermediate 4 and 5A molecular sieve is 10mmo l:30mmo l:2g.
[0075] The molar ratio of the intermediate 5, 2-aminoterephthalic acid and DOPO described in step B3 is 1:3:3, and the amount ratio of the organic ligand, samarium nitrate hexahydrate, N,N-dimethylformamide and deionized water is 1.5 mmol:1 mmol:50 mL:5 mL.
[0076] Comparative Example 1
[0077] Compared with Example 1, no modified monomer was added in this comparative example, and the remaining steps were the same.
[0078] Comparative Example 2
[0079] Compared with Example 1, this comparative example uses diamine-terminated polysiloxane instead of the modified monomer, and the remaining steps are the same.
[0080] Comparative Example 3
[0081] Compared with Example 1, this comparative example uses modified filler instead of functional filler, and the other steps are the same.
[0082] Comparative Example 4
[0083] Compared with Example 1, this comparative example did not add intermediate 5, and the remaining steps were the same.
[0084] The colored spun yarns obtained in Examples 1-3 and Comparative Examples 1-4 were made into samples of Condition A according to the standard of GB / T5455-2014, and the afterflaming time, smoldering time and damaged length were tested. The test results are shown in the following table.
[0085]
[0086] It can be seen from the above table that this application has a very good flame retardant effect.
[0087] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.
Claims
1. A method for preparing flame-retardant composite colored yarn, Features: The specific steps include: Step S1: mixing and stirring the modified filler, 3-isocyanatepropylmethyldimethoxysilane and toluene to obtain a functional filler, mixing and stirring 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, a modified monomer and N,N-dimethylacetamide and adding the functional filler to obtain a spinning solution; Step S2: keeping the temperature at high temperature to obtain reinforced fibers, dyeing the reinforced fibers respectively to obtain dyed fibers, opening, carding, drawing, roving and spinning the dyed fibers to obtain pretreated yarns, soaking the pretreated yarns in deionized water, taking them out and drying them to obtain flame-retardant composite colored spun yarns.
2. A method for preparing a flame-retardant composite color spun yarn according to claim 1, Features: The modified filler and 3-isocyanatepropylmethyldimethoxysilane described in step S1 are used in a ratio of 1 g:3 mL, and the ratio of 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, p-phenylenediamine, modified monomer, N,N-dimethylacetamide and functional filler is used in a ratio of 55 mmol:40 mmol:15 mmol:60 mL:5 g.
3. The method for preparing a flame-retardant composite colored spun yarn according to claim 1, Features: The modified monomer is prepared by the following steps: Step A1: phosphorus oxychloride, 2,2-dihydroxymethylpropionic acid and N,N-dimethylformamide are mixed and reacted to obtain intermediate 1, intermediate 1 is dissolved in N,N-dimethylformamide, nitrogen is introduced for protection, stirring and adding formic acid at a speed of 150-200 r / min and a temperature of 30-40° C., and reacting for 4-6 hours to obtain a phosphorus additive, phosphorus additive, KH550, dicyclohexylcarbodiimide and N,N-dimethylformamide are mixed, and reacting for 3-5 hours at a speed of 120-150 r / min and a temperature of 30-40° C. to obtain a phosphorus modifier; Step A2: octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane, tetramethylammonium hydroxide and dimethyl sulfoxide are mixed uniformly, nitrogen is introduced for protection, and the reaction is carried out for 3-5 hours at a speed of 120-150 r / min and a temperature of 90-100° C. to obtain a diamine-terminated polysiloxane; the diamine-terminated polysiloxane, a phosphorus modifier and N,N-dimethylformamide are mixed uniformly, nitrogen is introduced for protection, and the reaction is carried out for 40-45 hours at a speed of 150-200 r / min and a temperature of 65-70° C. to obtain a modified monomer.
4. A method for preparing a flame-retardant composite colored spun yarn according to claim 3, Features: The molar ratio of phosphorus oxychloride and 2,2-dihydroxymethylpropionic acid in step A1 is 1:1, the molar ratio of intermediate 1 and formic acid is 1:1, and the molar ratio of phosphorus additive, KH550 and dicyclohexylcarbodiimide is 1:1:1.
1.
5. The method for preparing a flame-retardant composite colored spun yarn according to claim 3, Features: The molar ratio of octamethylcyclotetrasiloxane, 2,4,6,8-tetravinyl-2,4,6,8-tetramethylcyclotetrasiloxane, 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and tetramethylammonium hydroxide described in step A2 is 1.8:0.6:2:3, and the molar ratio of the double bond on the diamine-terminated polysiloxane and the phosphorus modifier is 1:
1.
6. The method for preparing a flame-retardant composite colored spun yarn according to claim 1, Features: The modified filler is prepared by the following steps: Step B1: melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and methanol are mixed and stirred, and hydrochloric acid solution is added, and the temperature is raised to react to obtain intermediate 2; 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride ether and N,N-dimethylformamide are mixed and reacted, and sodium hydroxide solution is added, and the temperature is raised to react to obtain intermediate 3; Step B2: Mix and stir intermediate 3, sodium periodate, tetrahydrofuran and deionized water, add hydrochloric acid solution, and react to obtain intermediate 4; mix intermediate 2, intermediate 4, 5A molecular sieve and N,N-dimethylformamide to obtain intermediate 5; Step B3: After the intermediate 5, 2-aminoterephthalic acid and N,N-dimethylformamide are mixed and reacted, the pH is adjusted to be acidic, the temperature is increased and DOPO is added, and the reaction is continued to obtain an organic ligand. The organic ligand, samarium nitrate hexahydrate and N,N-dimethylformamide are mixed and stirred, and deionized water is added to react to obtain a modified filler.
7. A method for preparing a flame-retardant composite colored spun yarn according to claim 6, Features: The amount ratio of melamine, 3,4-dihydroxybenzaldehyde, 4A molecular sieve and hydrochloric acid solution in step B1 is 50mmol:150mmol:1g:2mL, and the amount ratio of 4-hydroxyphenylboronic acid pinacol ester, epichlorohydrin, boron trifluoride etherate and sodium hydroxide solution is 10mmol:10mmol:0.5g:30mL.
8. A method for preparing a flame-retardant composite colored spun yarn according to claim 6, Features: The amount ratio of intermediate 3, sodium periodate, tetrahydrofuran, deionized water and hydrochloric acid solution in step B2 is 5mmol:15mmol:40mL:10mL:3.5mL, and the amount ratio of intermediate 2, intermediate 4 and 5A molecular sieve is 10mmo l:30mmo l:2g.
9. A method for preparing a flame-retardant composite colored spun yarn according to claim 6, Features: The molar ratio of the intermediate 5, 2-aminoterephthalic acid and DOPO described in step B3 is 1:3:3, and the amount ratio of the organic ligand, samarium nitrate hexahydrate, N,N-dimethylformamide and deionized water is 1.5 mmol:1 mmol:50 mL:5 mL.
10. A flame retardant composite color spun yarn, Features: Prepared according to any one of claims 1 to 9.
Citation Information
Patent Citations
Composite yarn containing metal fiber and production process thereof
CN113249843A
Production process of non-woven fabric film coated copper flat wire
CN117854801A
Organic silicon-nitrogen flame-retardant regenerated cellulose fiber
EP3276053A1
IN2182CHN2013A