Metal nanolayer gain tri-coaxial structure photo-thermal aramid fiber and preparation method thereof
The nanometal and polydopamine layers are assembled on the surface of the aramid fiber through low-temperature plasma treatment and impregnation to form three-coaxial structure photothermal aramid fibers, which solves the problems of complex composite process and environmental pollution, and improves photothermal performance and resistance Tensile strength achieves green and economical production of photothermal materials.
Patent Information
- Application Number
- CN202411226757.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-11-19
AI Technical Summary
The prior art is difficult to effectively composite photothermal materials while maintaining high strength and high modulus of aramid fibers to improve their photothermal conversion performance. The existing method compounding process is complex, costly and pollution to the environment, and lacks effective improvement and Methods for regulating the efficiency of the photothermal layer.
The surface of aramid fiber is modified by low-temperature plasma treatment technology, and the nanometal layer and polydopamine layer are assembled on its surface by impregnation method to form a three-coaxial structure photothermal aramid fiber to improve the photothermal effect.
It has achieved a significant increase in the photothermal temperature and increased tensile strength under infrared light irradiation. It has a simple and environmentally friendly process, and is suitable for large-scale production, reducing production costs.
Smart Images

Figure CN118979379A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to an aramid fiber material and a preparation method thereof, and in particular to a metal nanolayer-gained tri-coaxial structure photothermal aramid fiber and a preparation method thereof. Background Art
[0002] In recent years, flexible photothermal materials have attracted widespread attention due to their potential applications in wearable electronic devices, photothermal drive systems, and smart textiles. For example, Lin Naibo et al. wet-spun a regenerated silk solution containing polydopamine nanoparticles into fibers, and coated the fibers with polydopamine. The fiber membrane prepared from the fibers showed good photothermal performance under laser irradiation and simulated sunlight, and has the potential to be used in flexible wearable electronic devices. In the prior art, LiYang, Luji Li, Junjie Lu, et al. Flexible Photothermal Materials with Controllable Accurate Healing and Reversible Adhesive Abilities. Macromolecules 2023, 56, 8, 3004-3014 dispersed true melanin into carboxyl styrene butadiene rubber to prepare a rubber elastomer with photothermal effect, which showed excellent near-infrared light-controlled healing ability. Daoguang Bi, Yangyang, Yingbang Yao, et al. Preparation and characterizations of flexible photothermal Ti2O3-PVA nancoomposites. Journal of Alloys and Compounds 2020, 825, 153998 Ti2O3 was surface modified and composited with a polyvinyl alcohol matrix to prepare a flexible photothermal nanocomposite film, which exhibited good flexibility and photothermal effect and is expected to be used in photothermal collection devices such as wearable electronic devices, solar-driven steam generators or seawater desalination devices.
[0003] Aramid fiber is a flexible fiber with high strength and high modulus. It has low density, high temperature resistance, chemical corrosion resistance, excellent flame retardancy and radiation resistance. It is widely used in bulletproof vests, aerospace, automotive industry, sports equipment, protective equipment and other fields. Considering the excellent performance of aramid fiber, if the photothermal material can be compounded with aramid fiber through reasonable material design, while maintaining the excellent properties of aramid fiber such as high strength and high modulus, it can be given a photothermal conversion effect to convert the absorbed light energy into heat energy. It is expected to be used for light-driven heating, temperature management, photothermal chemical reaction or integrated into smart textiles to achieve the regulation of the wearer's body temperature, providing a new direction for broadening the application range of aramid fiber.
[0004] There are still three difficulties in the preparation of photothermal aramid fibers. First, the surface of the aramid fibers needs to be reasonably treated and activated to improve the adhesion uniformity and stability of the photothermal layer. Second, in order to improve the production efficiency of photothermal aramid fibers, a simple and easy method needs to be selected to realize the composite of aramid fibers and the photothermal layer. At present, there are few studies and reports exploring how to solve the above two types of problems at the same time. Third, how to improve and regulate the photothermal efficiency of the photothermal layer on the surface of aramid fibers.
[0005] For the first problem, in order to improve the surface properties of aramid fibers, the commonly used methods currently include polymerization modification, chemical surface grafting and chemical etching to increase the surface polarity of aramid fibers. However, these chemical modification methods will inevitably damage the surface of aramid fibers, resulting in a decrease in their performance, and the waste liquid generated will pollute the environment. In recent years, physical modification methods such as low-temperature plasma treatment, ultraviolet irradiation grafting, ultrasonic treatment and high-energy ray treatment have been applied to the surface modification of aramid fibers. These methods can improve the surface properties of fibers through physical effects without destroying the fiber structure. Compared with physical modification methods such as ultraviolet irradiation grafting, ultrasonic treatment and high-energy ray treatment, low-temperature plasma treatment can modify the surface of large quantities of aramid fibers within tens of seconds, increase their surface activation energy and graft rich oxygen / nitrogen-containing functional groups, which is beneficial to improve the load uniformity and stability of the photothermal layer. In addition to its high efficiency, low-temperature plasma treatment technology does not produce polluting waste liquid, has almost no damage to the fibers, is green and environmentally friendly, and can maintain the original performance advantages of the fibers. In addition, the degree of surface modification of aramid fibers can be controlled by adjusting various technical parameters of low-temperature plasma.
[0006] For the second problem, at present, the method of loading functional substances on the surface of aramid fibers is mainly through electrospinning, chemical vapor deposition, in-situ polymerization, etc. Among them, methods such as electrospinning and chemical vapor deposition require the use of special equipment, and the production cost is relatively high and the process is complicated. In order to improve the production efficiency of photothermal aramid fibers and reduce production costs, it is necessary to select a simple and easy method to realize the composite of aramid fibers and photothermal layers. Compared with traditional electrospinning, chemical vapor deposition, in-situ polymerization and other technologies, the impregnation method usually does not require expensive equipment investment, has low production costs, simple process flow, easy operation, and can be applied to aramid fibers of various shapes and sizes, including yarns, fabrics, non-woven fabrics, etc., and has good applicability. In addition, by controlling the impregnation time and solution concentration, the amount and distribution of the loaded substance can be accurately controlled. Moreover, the impregnation method can not only be used to load a single functional substance, but also can achieve the composite loading of multiple substances by adjusting the formula of the impregnation solution. Therefore, the impregnation method can provide an economical, efficient, easy-to-operate and environmentally friendly solution for the loading of photothermal materials on the surface of aramid fibers. However, there are few studies and reports on the loading of photothermal materials on the surface of aramid fibers using the impregnation method.
[0007] The problem of how to improve and regulate the photothermal efficiency of the photothermal layer on the surface of aramid fibers can be solved by compounding a third phase material in the photothermal fibers. For example, in recent years, studies have shown that effects such as localized surface plasmon resonance (LSPR) of metal nanomaterials can enhance the photothermal conversion efficiency of photothermal polymers. However, related research mostly involves the fields of photocatalysis and biomedicine, and there are currently no reports on how to apply it to the fiber field to achieve the regulation of the photothermal effect of fibers such as aramid fibers as carriers. Summary of the invention
[0008] Purpose of the invention: The present invention aims to provide a tri-coaxial structure photothermal aramid fiber with metal nanolayer gain. The nano-metal layer can enhance the photothermal conversion effect of the photothermal polymer layer, and a synergistic photothermal effect is formed between the two to enhance the photothermal performance of the material. The second purpose of the present invention is to provide a preparation method of a tri-coaxial structure photothermal aramid fiber with metal nanolayer gain.
[0009] Technical solution: The three-coaxial structure photothermal aramid fiber with metal nanolayer gain described in the present invention comprises a photothermal polymer layer, a nanometal layer and aramid fiber, a bonding interface is formed between the nanometal layer and the surface of the aramid fiber, and a bonding interface is formed between the photothermal polymer layer and the nanometal layer.
[0010] Furthermore, the photothermal polymer is polydopamine, and the nanometal is nanogold or nanosilver.
[0011] Furthermore, the photothermal temperature of the photothermal aramid fiber under 100W to 300W infrared light irradiation is 120 to 150°C, and the tensile strength is 1300 to 1600MPa.
[0012] The preparation method of the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain comprises: using the plasma-treated aramid fiber as a carrier, and sequentially assembling a nanometal layer and a polydopamine layer on the surface of the aramid fiber.
[0013] Furthermore, the plasma radio frequency power is 100W to 200W, the processing time is set to 30 seconds to 180 seconds, and the added gas is one of air or oxygen.
[0014] Furthermore, the plasma-treated aramid fiber is immersed in a dispersion containing nano-metal particles, and the nano-metal particles self-assemble on the surface of the plasma-treated aramid fiber to form a nano-metal layer; the aramid fiber assembled with the nano-metal layer is immersed in a dopamine hydrochloride solution containing tris(hydroxymethyl)aminomethane, and dopamine hydrochloride polymerizes on the surface of the nano-metal layer to form a polydopamine layer.
[0015] Furthermore, the preparation method of the dispersion containing nano-metal particles comprises: adding the aqueous solution containing HAuCl4 or CH3COOAg dropwise into the boiling sodium citrate aqueous solution, heating and stirring for 15 minutes to 30 minutes. Furthermore, the aramid fiber is immersed in the aqueous dispersion of the nano-metal for 24 hours to 96 hours, and the aramid fiber assembled with the nano-metal is immersed in the dopamine hydrochloride solution for 24 hours to 96 hours.
[0016] Furthermore, in the dopamine hydrochloride solution, the concentration of tris(hydroxymethyl)aminomethane is 0.1M to 1M, the concentration of dopamine hydrochloride is 0.05 to 0.1M, and the pH value is 8.8 to 9.0.
[0017] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in the present invention forms a bonding interface between the nanometal layer and the surface of the aramid fiber, and a bonding interface between the photothermal polymer layer and the nanometal layer. This structure forms a synergistic photothermal effect between the nanometal layer and the photothermal polymer layer; under 100W to 300W infrared light irradiation, the temperature of the coaxial aramid fiber can reach 144°C. Compared with aramid fiber, the photothermal temperature of the three-coaxial structure photothermal aramid fiber is increased by 81°C; compared with the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without nanometal layer and with polydopamine photothermal polymer layer, the photothermal temperature of the three-coaxial structure photothermal aramid fiber is increased by 37°C; in addition, the tensile strength of the coaxial photothermal aramid fiber can reach 1503MPa, which is higher than that of similar fibers.
[0018] Beneficial effects: Compared with the prior art, the present invention has the following significant advantages:
[0019] (1) A three-coaxial structure of "photothermal polymer layer / nanometal layer / aramid fiber" was constructed with aramid fiber as the core and nanometal layer and photothermal polymer layer as the shell. The nanometal layer can enhance the photothermal conversion effect of the photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which can increase the photothermal temperature under infrared light irradiation by 37°C.
[0020] (2) Rapid low-temperature plasma surface treatment technology is used to treat and modify the aramid fiber surface. Rich oxygen-containing functional groups, nitrogen-containing functional groups and other active functional groups are grafted onto the aramid fiber surface and the surface activation energy is increased. This can effectively improve the bonding strength and distribution uniformity of nano-metals on the aramid fiber surface. The tensile strength of the photothermal aramid fiber can reach 1503MPa, which is higher than that of similar fibers.
[0021] (3) The impregnation treatment technology is used to achieve the self-assembly of the nano-metal layer on the surface of the aramid fiber and the polymerization and assembly of the dopamine layer on the surface of the nano-metal layer. The method is simple and easy to use, and can be used to treat large quantities of aramid fibers to achieve large-scale production. It will not cause damage to the internal structure of the fiber, and no corrosive waste liquid will be generated, thus achieving green production. In addition, by adjusting the impregnation parameters (time, concentration, pH value, etc.), the assembly conditions of the metal nano-layer and the polydopamine layer on the surface of the aramid fiber (such as layer thickness, degree of polymerization, etc.) can be controlled. BRIEF DESCRIPTION OF THE DRAWINGS
[0022] Figure 1 This is a schematic diagram of the structure of the photothermal aramid fiber with a three-coaxial structure of “photothermal polymer layer / nano-gold layer / aramid fiber” of Example 1;
[0023] Figure 2 This is a force-displacement curve of the photothermal aramid fiber with a three-coaxial structure of "photothermal polymer layer / nanosilver layer / aramid fiber" in Example 1;
[0024] Figure 3 This is the force-displacement curve of the “photothermal polymer layer / nano-gold layer / aramid fiber” tri-coaxial structure photothermal aramid fiber of Example 2;
[0025] Figure 4 This is a schematic diagram of the composite fiber structure of Comparative Example 3. DETAILED DESCRIPTION
[0026] The technical solution of the present invention is further described below in conjunction with the accompanying drawings.
[0027] Example 1
[0028] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in this embodiment uses the plasma-treated aramid fiber as a carrier, the nanosilver layer is coated on the surface of the aramid fiber, and the photothermal polymer layer (polydopamine layer) is coated on the surface of the nanosilver layer to form a coaxial structure. A bonding interface is formed between the nanosilver layer and the surface of the aramid fiber, and a bonding interface is formed between the polymer layer (polydopamine layer) with photothermal effect and the nanosilver layer. The structure is shown in the attached figure. Figure 1 shown.
[0029] The specific preparation method is as follows:
[0030] (1) A 0.0001 M CH3COOAg aqueous solution was added dropwise into a boiling 0.01 M sodium citrate aqueous solution at 96° C. with magnetic stirring for 15 min to prepare an aqueous dispersion of nanosilver particles.
[0031] (2) Aramid fibers were treated with low-temperature plasma, the plasma radio frequency power was 150 W, the treatment time was 90 seconds, and the external gas was air.
[0032] (3) The aramid fiber is immersed in the aqueous dispersion of the nanosilver particles and allowed to stand for 24 hours, and the nanosilver particles are self-assembled on the surface of the aramid fiber to form a nanosilver layer.
[0033] (4) The aramid fiber with the nanosilver layer assembled on the surface is placed at 80° C. and vacuum dried.
[0034] (5) The dried aramid fiber with the silver nanoparticle layer assembled on the surface was immersed in a tris buffer solution of dopamine hydrochloride at a pH of 8.8 and allowed to stand for 24 hours. The concentration of tris(hydroxymethyl)aminomethane in the solution was 1 M, and the concentration of dopamine hydrochloride was 0.062 M.
[0035] (6) During the static process, dopamine hydrochloride molecules self-polymerize and assemble on the surface of the nanosilver layer to form a tri-coaxial aramid fiber of “aramid fiber / nanosilver layer / polydopamine polymer layer”.
[0036] (7) The coaxial aramid fibers were placed at 70°C and vacuum dried.
[0037] (8) The photothermal effect of the above coaxial aramid fiber under infrared light irradiation was tested, and the infrared light power was 275W.
[0038] The test results show that the photothermal temperature of the three-coaxial structure photothermal aramid fiber of the embodiment of the present invention, which uses the metal nanolayer gain photothermal conversion effect, is as high as 136°C.
[0039] The mechanical properties of the coaxial photothermal aramid fiber are tested, and the force-displacement curve is shown in Figure 2 As shown, its tensile strength reaches 1354MPa.
[0040] Comparative Example 1
[0041] Under 275W infrared light irradiation, the photothermal temperature of the aramid fiber without the nano-gold layer and the polydopamine photothermal polymer layer reached 63°C. In comparison, the photothermal temperature of the triaxial structure photothermal aramid fiber of Example 1 increased by 73°C.
[0042] Comparative Example 2
[0043] Under 275W infrared light irradiation, the photothermal temperature of the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without nanosilver layer and with polydopamine photothermal polymer layer reached 100°C. In comparison, the photothermal temperature of the three coaxial structure photothermal aramid fiber of Example 1 increased by 36°C.
[0044] The above test results show that the nano-gold layer enhances the photothermal conversion effect of the polydopamine photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which jointly increase the temperature of the fiber material under infrared light irradiation.
[0045] Comparative Example 3
[0046] The aramid fiber is used as the core, and a polydopamine photothermal polymer layer embedded with silver nanoparticles is assembled on its surface. Figure 4 As shown, the preparation method is as follows:
[0047] A 0.0001M CH3COOAg aqueous solution was added dropwise into a boiling 0.01M sodium citrate aqueous solution at 96°C with magnetic stirring for 15 minutes to prepare an aqueous dispersion of nanosilver particles.
[0048] Tris(hydroxymethyl)aminomethane was added to the aqueous dispersion of the nanosilver particles until the concentration was 1 M, and the pH value was adjusted to 8.8. Dopamine hydrochloride was then added and ultrasonic dispersion was performed.
[0049] The aramid fiber was treated with low-temperature plasma, the plasma radio frequency power was 150 W, the treatment time was 90 seconds, and the external gas was air.
[0050] The aramid fiber treated with low-temperature plasma was immersed in the above-mentioned tris buffer dispersion containing dopamine hydrochloride and nano-silver particles and allowed to stand for 24 hours.
[0051] During the static process, dopamine hydrochloride molecules self-polymerize to form polydopamine and assemble on the surface of aramid fiber. The silver nanoparticles are encapsulated and embedded in the polydopamine polymer layer. However, the silver nanolayer and aramid fiber do not form a coating structure. There is no bonding interface between the two, and they do not form a "photothermal polymer layer / nanometallic layer / aramid fiber" triaxial structure. Its structure is shown in the attached figure. Figure 4 shown.
[0052] The aramid fiber was placed at 80°C and vacuum dried.
[0053] The photothermal effect of the coaxial aramid fiber was tested under infrared light irradiation. The infrared light power was 275W, and the photothermal temperature of the composite aramid fiber was 107°C.
[0054] The photothermal temperature of the photothermal aramid fiber described in Comparative Example 3 is 107°C, and Example 1 is 29°C higher than Comparative Example 3. This result shows that the three-coaxial structure with a silver nanolayer as the intermediate layer described in the present invention has a significant effect on enhancing its photothermal effect.
[0055] Example 2
[0056] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in this embodiment uses the plasma-treated aramid fiber as a carrier, the nanogold layer is coated on the surface of the aramid fiber, and the photothermal polymer layer (polydopamine layer) is coated on the surface of the nanogold layer to form a coaxial structure. A bonding interface is formed between the nanogold layer and the surface of the aramid fiber, and a bonding interface is formed between the polymer layer (polydopamine layer) with photothermal effect and the nanogold layer. The structure is shown in the attached figure. Figure 1 shown.
[0057] The specific preparation method is as follows:
[0058] (1) A 0.0001 M HAuCl4 aqueous solution was added dropwise into a boiling 0.01 M sodium citrate aqueous solution at 96°C with magnetic stirring for 15 min to prepare an aqueous dispersion of gold nanoparticles.
[0059] (2) Aramid fibers were treated with low-temperature plasma, the plasma radio frequency power was 120 W, the treatment time was 90 seconds, and the external gas was air.
[0060] (3) The aramid fiber treated with low-temperature plasma was immersed in the aqueous dispersion of the nano-gold particles and allowed to stand for 96 hours, and the nano-gold particles self-assembled on the surface of the aramid fiber to form a nano-gold layer.
[0061] (4) The aramid fiber with the gold nanoparticles assembled on its surface was placed at 80° C. and dried in vacuum.
[0062] (5) The dried aramid fiber with the gold nanoparticles assembled on its surface was immersed in a tris buffer solution of dopamine hydrochloride at a pH of 8.8 and allowed to stand for 96 hours. The concentration of tris(hydroxymethyl)aminomethane in the solution was 1 M, and the concentration of dopamine hydrochloride was 0.062 M.
[0063] (6) During the static process, dopamine hydrochloride molecules self-polymerize and assemble on the surface of the nano-gold layer to form a tri-coaxial aramid fiber of “aramid fiber / nano-gold layer / polydopamine polymer layer”.
[0064] (7) The coaxial aramid fibers were placed at 80°C and vacuum dried.
[0065] (8) The photothermal effect of the above coaxial aramid fiber under infrared light irradiation was tested, and the infrared light power was 275W.
[0066] The test results show that:
[0067] The photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment, which uses the metal nanolayer gain photothermal conversion effect, reaches 144°C. Compared with comparative example 1, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment is increased by 81°C.
[0068] The mechanical properties of the above coaxial aramid fiber photothermal aramid fiber are tested, and the force-displacement curve is shown in the figure below. Figure 3 As shown, its tensile strength reaches 1503MPa.
[0069] Comparative Example 4
[0070] Under 275W infrared light irradiation, the photothermal temperature of the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without the nano-gold layer and with the polydopamine photothermal polymer layer reached 107°C. In comparison, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of Example 2 increased by 37°C.
[0071] The above test results show that the nano-gold layer enhances the photothermal conversion effect of the polydopamine photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which jointly increase the temperature of the fiber material under infrared light irradiation.
[0072] Example 3
[0073] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in this embodiment uses the plasma-treated aramid fiber as a carrier, the nanogold layer is coated on the surface of the aramid fiber, and the photothermal polymer layer (polydopamine layer) is coated on the surface of the nanogold layer to form a coaxial structure. A bonding interface is formed between the nanogold layer and the surface of the aramid fiber, and a bonding interface is formed between the polymer layer (polydopamine layer) with photothermal effect and the nanogold layer.
[0074] The specific preparation method is as follows:
[0075] (1) A 0.0001 M HAuCl4 aqueous solution was added dropwise into a boiling 0.01 M sodium citrate aqueous solution at 96°C with magnetic stirring for 15 min to prepare an aqueous dispersion of gold nanoparticles.
[0076] (2) Aramid fibers were treated with low-temperature plasma, the plasma radio frequency power was 100 W, the treatment time was 120 seconds, and the external gas was air.
[0077] (3) The aramid fiber treated with low-temperature plasma was immersed in the aqueous dispersion of the nano-gold particles and allowed to stand for 96 hours, and the nano-gold particles self-assembled on the surface of the aramid fiber to form a nano-gold layer.
[0078] (4) The aramid fiber with the gold nanoparticles assembled on its surface was placed at 90° C. and dried in vacuum.
[0079] (5) The dried aramid fiber with the gold nanoparticles assembled on its surface was immersed in a tris buffer solution of dopamine hydrochloride and allowed to stand for 48 hours, wherein the concentration of tris(hydroxymethyl)aminomethane in the solution was 1 M, and the concentration of dopamine hydrochloride was 0.062 M.
[0080] (6) During the static process, dopamine hydrochloride molecules self-polymerize and assemble on the surface of the nano-gold layer to form a tri-coaxial aramid fiber of “aramid fiber / nano-gold layer / polydopamine polymer layer”.
[0081] (7) The coaxial aramid fibers are placed at 90°C and vacuum dried.
[0082] (8) The photothermal effect of the test material under infrared light irradiation, the infrared light power is 275W.
[0083] The test results show that:
[0084] The photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment, which uses the metal nanolayer gain photothermal conversion effect, reaches 127° C. Compared with comparative example 1, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment is increased by 64° C.
[0085] Comparative Example 5
[0086] Under 275W infrared light irradiation, the photothermal temperature of the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without the nano-gold layer and with the polydopamine photothermal polymer layer reached 104°C. In comparison, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of Example 3 increased by 23°C.
[0087] The above test results show that the nano-gold layer enhances the photothermal conversion effect of the polydopamine photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which jointly increase the temperature of the fiber material under infrared light irradiation.
[0088] Example 4
[0089] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in this embodiment uses the plasma-treated aramid fiber as a carrier, the nanogold layer is coated on the surface of the aramid fiber, and the photothermal polymer layer (polydopamine layer) is coated on the surface of the nanogold layer to form a coaxial structure. A bonding interface is formed between the nanogold layer and the surface of the aramid fiber, and a bonding interface is formed between the polymer layer (polydopamine layer) with photothermal effect and the nanogold layer.
[0090] The specific preparation method is as follows:
[0091] (1) A 0.0001 M HAuCl4 aqueous solution was added dropwise into a boiling 0.01 M sodium citrate aqueous solution at 96°C with magnetic stirring for 15 min to prepare an aqueous dispersion of gold nanoparticles.
[0092] (2) Aramid fibers were treated with low-temperature plasma, the plasma radio frequency power was 100 W, the treatment time was 120 seconds, and the external gas was air.
[0093] (3) The aramid fiber treated with low-temperature plasma was immersed in the aqueous dispersion of the nano-gold particles and allowed to stand for 96 hours, and the nano-gold particles self-assembled on the surface of the aramid fiber to form a nano-gold layer.
[0094] (4) The aramid fiber with the gold nanoparticles assembled on its surface was placed at 60° C. and vacuum dried.
[0095] (5) The dried aramid fiber with the gold nanoparticles assembled on its surface was immersed in a tris buffer solution of dopamine hydrochloride at a pH of 8.8 and allowed to stand for 24 hours. The concentration of tris(hydroxymethyl)aminomethane in the solution was 1 M, and the concentration of dopamine hydrochloride was 0.062 M.
[0096] (6) During the static process, dopamine hydrochloride molecules self-polymerize and assemble on the surface of the nano-gold layer to form a tri-coaxial aramid fiber of “aramid fiber / nano-gold layer / polydopamine polymer layer”.
[0097] (7) The coaxial aramid fibers were placed at 60°C and vacuum dried.
[0098] (8) The photothermal effect of the above coaxial aramid fiber under infrared light irradiation was tested, and the infrared light power was 275W.
[0099] The test results show that:
[0100] The photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment, which uses the metal nanolayer gain photothermal conversion effect, reaches 121° C. Compared with comparative example 1, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of the present embodiment is increased by 58° C.
[0101] Comparative Example 6
[0102] Under 275W infrared light irradiation, the photothermal temperature of the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without the nano-gold layer and with the polydopamine photothermal polymer layer reached 100°C. In comparison, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of Example 4 increased by 21°C.
[0103] The above test results show that the nanosilver layer enhances the photothermal conversion effect of the polydopamine photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which jointly increase the temperature of the fiber material under infrared light irradiation.
[0104] Example 5
[0105] The three-coaxial structure photothermal aramid fiber of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain described in this embodiment uses the plasma-treated aramid fiber as a carrier, the nanogold layer is coated on the surface of the aramid fiber, and the photothermal polymer layer (polydopamine layer) is coated on the surface of the nanogold layer to form a coaxial structure. A bonding interface is formed between the nanogold layer and the surface of the aramid fiber, and a bonding interface is formed between the polymer layer (polydopamine layer) with photothermal effect and the nanogold layer.
[0106] The specific preparation method is as follows:
[0107] (1) A 0.0001 M HAuCl4 aqueous solution was added dropwise into a boiling 0.01 M sodium citrate aqueous solution at 96°C with magnetic stirring for 15 min to prepare an aqueous dispersion of gold nanoparticles.
[0108] (2) Aramid fibers were treated with low-temperature plasma, the plasma radio frequency power was 120 W, the treatment time was 60 seconds, and the external gas was air.
[0109] (3) The aramid fiber treated with low-temperature plasma is immersed in the aqueous dispersion of the above-mentioned nano-gold particles and allowed to stand for 48 hours. The nano-gold particles self-assemble on the surface of the aramid fiber to form a nano-gold layer.
[0110] (4) The aramid fiber with the gold nanoparticles assembled on its surface was placed at 70° C. and vacuum dried.
[0111] (5) The dried aramid fiber with the gold nanoparticles assembled on the surface was immersed in a tris buffer solution of dopamine hydrochloride for 96 hours, wherein the concentration of tris(hydroxymethyl)aminomethane in the solution was 1 M, and the concentration of dopamine hydrochloride was 0.062 M.
[0112] (6) During the static process, dopamine hydrochloride molecules self-polymerize and assemble on the surface of the nano-gold layer to form a tri-coaxial aramid fiber of “aramid fiber / nano-gold layer / polydopamine polymer layer”.
[0113] (7) The coaxial aramid fibers were placed at 70°C and vacuum dried.
[0114] (8) The photothermal effect of the test material under infrared light irradiation, the infrared light power is 275W.
[0115] The test results show that:
[0116] The photothermal temperature of the photothermal aramid fiber with a three-coaxial structure of "photothermal polymer layer / nanometal layer / aramid fiber" with the photothermal conversion effect of the metal nanolayer gain reaches 121°C.
[0117] Compared with Comparative Example 1, the photothermal temperature of the tri-coaxial structure photothermal aramid fiber of this embodiment is increased by 58°C.
[0118] Comparative Example 7
[0119] Under 275W infrared light irradiation, the photothermal temperature of the coaxial structure aramid fiber of "photothermal polymer layer / aramid fiber" without the nano-gold layer and with the polydopamine photothermal polymer layer reached 107°C. In comparison, the photothermal temperature of the three-coaxial structure photothermal aramid fiber of Example 5 increased by 14°C.
[0120] The above test results show that the nano-gold layer enhances the photothermal conversion effect of the polydopamine photothermal polymer layer, and a synergistic photothermal effect is formed between the two, which jointly increase the temperature of the fiber material under infrared light irradiation.
Claims
1. A triaxial photothermal aramid fiber with metal nanolayer gain. It is characterized in that The triaxial structure of the photothermal aramid fiber is composed of a photothermal polymer layer, a nanometal layer and aramid fiber. A bonding interface is formed between the nanometal layer and the surface of the aramid fiber, and a bonding interface is formed between the photothermal polymer layer and the nanometal layer.
2. The tri-coaxial structured photothermal aramid fiber with metal nanolayer gain according to claim 1, It is characterized in that The photothermal polymer is polydopamine, and the nanometal is nanogold or nanosilver.
3. The tri-coaxial structured photothermal aramid fiber with metal nanolayer gain according to claim 1, It is characterized in that The photothermal temperature of the photothermal aramid fiber under 100W-300W infrared light irradiation is 120-150°C, and the tensile strength is 1300-1600MPa.
4. A method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to any one of claims 1 to 3, It is characterized in that The method comprises: using plasma-treated aramid fiber as a carrier, and sequentially assembling a nano metal layer and a polydopamine layer on the surface of the aramid fiber.
5. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 4, It is characterized in that The plasma radio frequency power is 100W to 200W, the processing time is set to 30 seconds to 180 seconds, and the added gas is one of air or oxygen.
6. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 4, It is characterized in that The plasma-treated aramid fiber is immersed in a dispersion containing nano-metal particles, and the nano-metal particles are self-assembled on the surface of the plasma-treated aramid fiber to form a nano-metal layer.
7. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 4, It is characterized in that The aramid fiber assembled with the nano-metal layer is immersed in a dopamine hydrochloride solution containing tris(hydroxymethyl)aminomethane, and the dopamine hydrochloride is polymerized on the surface of the nano-metal layer to form a polydopamine layer.
8. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 6, It is characterized in that The preparation method of the dispersion containing nano metal particles comprises: 4 or CH 3 The COOAg aqueous solution was added dropwise into the boiling sodium citrate aqueous solution, and heated with stirring for 15 min to 30 min.
9. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 4, It is characterized in that The aramid fiber is immersed in the aqueous dispersion of the nano-metal for 24 hours to 96 hours, and the aramid fiber assembled with the nano-metal is immersed in the dopamine hydrochloride solution for 24 hours to 96 hours.
10. The method for preparing the tri-coaxial structure photothermal aramid fiber with metal nanolayer gain according to claim 7, It is characterized in that In the dopamine hydrochloride solution, the concentration of tris(hydroxymethyl)aminomethane is 0.1M-1M, the concentration of dopamine hydrochloride is 0.05-0.1M, and the pH value is 8.8-9.0.