All-geopolymer prefabricated wall integrating heat preservation, heat insulation and double fire prevention
By using prefabricated walls made entirely of geological polymer materials and with a combined design, the problem of traditional prefabricated walls being prone to failure under fire conditions has been solved, achieving excellent thermal insulation, fire resistance, and environmental protection performance, and providing dual economic and environmental benefits.
Patent Information
- Application Number
- CN202411050440.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-01
- Publication Date
- 2024-11-19
AI Technical Summary
Existing precast walls are prone to failure under fire conditions, and traditional insulation materials have problems such as the release of toxic gases, poor impact resistance, and insufficient environmental performance.
Prefabricated walls with thermal insulation, heat insulation, and dual fire resistance are made using all-geopolymer materials. The combination design of C-shaped ceramic splicing fireproof boards, crack-resistant insulation layers, and inorganic shear-resistant connectors ensures connection stability and fire resistance at high temperatures.
It achieves excellent thermal insulation, dual fire resistance, impact resistance, and green environmental protection characteristics, solving the fire resistance and environmental protection problems of traditional precast walls and providing both economic and environmental benefits.
Smart Images

Figure CN118979570A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of prefabricated walls, and in particular to a full-geopolymer prefabricated wall integrating thermal insulation, heat insulation and double fire protection. Background Art
[0002] Prefabricated buildings are the future development direction of my country's construction industry, and prefabricated walls are one of the core components of prefabricated buildings. Sandwich structures with insulation layers are common structural forms of prefabricated walls. However, the insulation materials in sandwich structures are usually organic materials, which will release toxic gases under fire conditions; moreover, such insulation materials usually have poor impact resistance, resulting in serious damage to the exterior walls under accidental impact; in addition, ordinary silicate concrete will burst during indoor fires, causing damage to the walls. Furthermore, cement and organic insulation boards will also produce a large amount of carbon dioxide during the production process, which runs counter to the "dual carbon" goal advocated by my country.
[0003] Geopolymer is a cementitious material made from industrial solid waste, which has the characteristics of high temperature resistance, environmental protection, low thermal conductivity and high performance. In order to promote the development of prefabricated buildings, geopolymer can be used to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a full geopolymer prefabricated wall that integrates thermal insulation, heat insulation and dual fire protection, which can well solve the problem of failure of silicate cement, organic thermal insulation wall panels and metal connectors used in the prior art sandwich prefabricated walls at high temperatures, and meet the comprehensive needs of thermal insulation, heat insulation, fire protection and greenness of prefabricated walls.
[0005] In order to achieve the above object, the present invention adopts the following technical solutions:
[0006] The present invention provides a fully geopolymer prefabricated wall integrating thermal insulation, heat insulation and double fire protection, comprising a base wall, one side of the base wall is connected to a C-shaped ceramic splicing fireproof board, and the other side of the base wall is connected to an anti-cracking thermal insulation layer; the upper and lower ends of the C-shaped ceramic splicing fireproof board are respectively provided with an upper extension plate and a lower extension plate which are clamped and fixed to the base wall, the anti-cracking thermal insulation layer is connected to the base wall through an inorganic shear-resistant connector, and the base wall is provided with a reserved channel for riveting the inorganic shear-resistant connector on a surface of one side facing the anti-cracking thermal insulation layer, and the gap between the reserved channel and the inorganic shear-resistant connector is filled with a sealing inorganic glue.
[0007] Furthermore, the anti-crack and heat-insulating layer comprises an anti-crack and fire-proof layer and a heat-insulating and heat-insulating layer, wherein the heat-insulating and heat-insulating layer is prepared from foam-modified geopolymer, and the anti-crack and fire-proof layer is prepared from fiber woven mesh reinforced inorganic resin mortar.
[0008] Furthermore, the inorganic resin mortar is formed by uniformly mixing inorganic resin and quartz sand in a mass ratio of 1:1.25.
[0009] Furthermore, the fiber woven mesh is at least one of a basalt fiber woven mesh, a carbon fiber woven mesh, and a glass fiber woven mesh.
[0010] Furthermore, the fiber braided mesh is evenly arranged in several layers, and the interval between the fiber braided meshes is 1 to 3 mm.
[0011] Furthermore, the anti-crack insulation layer is in the shape of a rectangular plate, the width of a single anti-crack insulation layer is ≤1200mm, the height is ≤600mm, and the thickness is 50-100mm. The thickness of the anti-crack fireproof layer is 5mm-8mm, and the thickness of the thermal insulation layer is 45mm-72mm.
[0012] Furthermore, the C-type ceramic spliced fireproof board is formed by using continuous fiber roving to reinforce inorganic resin through resin transfer molding.
[0013] Furthermore, the continuous fiber roving is at least one of basalt fiber, carbon fiber and glass fiber.
[0014] Furthermore, the volume of the continuous fiber roving accounts for 40% to 50% of the volume of the C-type ceramic spliced fireproof board.
[0015] Furthermore, the inorganic resin is a ceramic geopolymer. As an example, a commercial ceramic geopolymer matrix MEYEB can be used.
[0016] Furthermore, the thickness of the C-type ceramic spliced fireproof board is 10 to 15 mm, and the lengths of the upper extension board and the lower extension board in the direction perpendicular to the C-type ceramic spliced fireproof board are not less than 20 mm.
[0017] Furthermore, the inorganic shear-resistant connector is composed of a connected screw portion and a nut portion, and the inorganic shear-resistant connector includes an embedded reinforcement layer located inside and an external insulation layer wrapped around the outer periphery of the embedded reinforcement layer; the embedded reinforcement layer is obtained by compression molding using mini FRP bars to reinforce inorganic resin; the external insulation layer is prepared by molding using foam-modified polymer.
[0018] Furthermore, the foam-modified geopolymer is a slurry obtained by stirring and mixing sodium silicate solution, low-calcium fly ash, foaming agent and water in a mass ratio of 8:7:(1.9-3.8):5.
[0019] Furthermore, the foaming agent is any one of hollow glass microspheres, silica aerogel, and protein foaming agent.
[0020] Furthermore, the mini FRP bar is at least one of BFRP bar (basalt fiber), CFRP bar (carbon fiber) and GFRP bar (glass fiber).
[0021] Furthermore, the length of the mini FRP rib is 10 mm smaller than the diameter of the screw portion, and the diameter of the mini FRP rib is 1 / 40 to 1 / 50 of the length of the mini FRP rib.
[0022] Furthermore, the mini FRP bars are arranged in three rows along the circumferential direction in the embedded reinforcement layer, the spacing between each row of mini FRP bars is one quarter of the diameter of the embedded reinforcement layer, the number of mini FRP bars in the outermost row is not less than 8, the number of mini FRP bars in the middle row is not less than 4, and the number of mini FRP bars in the innermost row is not less than 1.
[0023] Furthermore, the length of the inorganic shear-resistant connector is the sum of the thickness of the anti-cracking insulation layer plus the anchoring depth of not less than 50 mm; the diameter of the screw portion is 25 to 40 mm; the diameter of the nut portion is not less than 50 mm, and the thickness of the nut portion is 1 / 4 to 1 / 2 of the diameter of the nut portion; the diameter of the embedded reinforcement layer is 20 to 35 mm; the thickness of the external insulation layer is 5 to 10 mm; the shear strength of the inorganic shear-resistant connector is not less than 50% of its tensile strength.
[0024] Furthermore, the base wall is built using geopolymer mortar masonry bricks.
[0025] Further, the preparation method of geopolymer mortar masonry brick is as follows: Sodium silicate solution with modulus 2.3, S105 slag and quartz sand fine aggregate are uniformly stirred at a mass ratio of 1:1.25:1.5 by a mechanical stirrer at room temperature-atmosphere environment for 5 minutes to obtain geopolymer mortar, and the obtained geopolymer mortar is injected into a masonry brick mold of standard size, and after standard curing (20±2℃, 97%RH) for 28 days, a geopolymer mortar masonry brick is obtained. The compressive strength of the geopolymer mortar masonry brick is 33MPa.
[0026] Furthermore, no less than 4 of the reserved channels are provided per square meter on the side surface of the base wall.
[0027] Furthermore, the diameter of the reserved channel is 3 mm larger than the diameter of the screw portion of the inorganic shear-resistant connector; and the depth of the reserved channel is greater than 50 mm.
[0028] Furthermore, the sealing inorganic glue is a geopolymer slurry obtained by uniformly mechanically stirring a sodium silicate solution with a modulus of 2.3 and S105 slag at a mass ratio of 1:1.25 at room temperature. After 28 days of standard curing, the compressive strength is not less than 50 MPa.
[0029] Compared with the prior art, the present invention provides a geopolymer prefabricated wall that integrates thermal insulation, heat insulation and double fire protection, and has the following beneficial effects:
[0030] The all-geopolymer prefabricated wall provided by the present invention has the advantages of good thermal insulation effect, dual fire protection indoors and outdoors, good impact resistance, purely mechanized construction, green environmental protection, etc., and well solves the problems of traditional sandwich insulation walls such as poor impact resistance, single-sided fire protection, and easy shedding of the insulation layer, thereby achieving dual benefits of economy and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0032] Figure 1 It is a structural schematic diagram of the present invention;
[0033] Figure 2 for Figure 1 The enlarged schematic diagram at A in the middle;
[0034] Figure 3 This is a schematic diagram of the structure of a C-type ceramic spliced fireproof board;
[0035] Figure 4 It is a structural schematic diagram of the anti-cracking thermal insulation layer;
[0036] Figure 5 It is a schematic diagram of the three-dimensional structure of an inorganic shear-resistant connector;
[0037] Figure 6 It is a schematic diagram of a half-section structure of an inorganic shear connector;
[0038] Figure 7 for Figure 6 Cross-section along the BB direction.
[0039] Figure numerals: 1. Base wall; 11. Reserved channel; 2. C-type ceramic splicing fireproof board; 21. Upper extension board; 22. Lower extension board; 23. Continuous fiber roving; 3. Anti-crack insulation layer; 31. Anti-crack fireproof layer; 32. Thermal insulation layer; 33. Fiber woven mesh; 4. Inorganic shear connector; 41. Screw part; 42. Nut part; 43. Embedded reinforcement layer; 44. Outer insulation layer; 45. Mini FRP ribs; 5. Sealing inorganic glue. DETAILED DESCRIPTION
[0040] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0041] refer to Figure 1 to Figure 7 The present invention provides a fully geopolymer prefabricated wall that integrates heat preservation, thermal insulation, and dual fire protection, including a base wall 1, one side of the base wall 1 is connected to a C-type ceramic splicing fireproof board 2, and the other side of the base wall 1 is connected to an anti-cracking thermal insulation layer 3; the upper and lower ends of the C-type ceramic splicing fireproof board 2 are respectively provided with an upper extension plate 21 and a lower extension plate 22 that are clamped and fixed to the base wall 1, and the anti-cracking thermal insulation layer 3 is connected to the base wall 1 through an inorganic shear connector 4. The base wall 1 is provided with a reserved channel 11 for riveting the inorganic shear connector 4 on the side surface facing the anti-cracking thermal insulation layer 3, and the pores between the reserved channel 11 and the inorganic shear connector 4 are filled with a sealing inorganic glue 5. The inorganic shear connector is installed in the reserved channel and sealed with a sealing inorganic glue to achieve a reliable connection between the base wall and the anti-cracking thermal insulation layer, and the use of an inorganic shear connector can well avoid the problem of connection failure under high temperature in a fire. By setting C-shaped ceramic splicing fireproof panels and anti-cracking insulation layers on both sides of the base wall, it has the advantages of good insulation effect, double fire protection indoors and outdoors, good impact resistance, purely mechanized construction, and green environmental protection. It solves the problems of traditional sandwich insulation walls such as impact resistance, single-sided fire protection, and easy falling off of the insulation layer, and achieves both economic and environmental benefits.
[0042] Among them, reference Figure 4 , the anti-crack thermal insulation layer 3 includes an anti-crack fireproof layer 31 and a thermal insulation layer 32. The thermal insulation layer 32 is made of foam-modified geopolymer and has good thermal insulation and heat insulation effects. The anti-crack fireproof layer 31 is made of fiber woven mesh 33 reinforced inorganic resin mortar and has good crack resistance. In some specific embodiments, the inorganic resin mortar is formed by uniformly mixing inorganic resin and quartz sand in a mass ratio of 1:1.25. The fiber woven mesh 33 can be selected from at least one of basalt fiber woven mesh, carbon fiber woven mesh, and glass fiber woven mesh. The fiber woven mesh 33 is evenly arranged in several layers, and the spacing distance of the fiber woven mesh 33 is 1 to 3 mm. The fiber woven mesh is evenly coated on the surface with acrylic resin before use, and is pressed and shaped using a flat plate. As an example, the anti-crack thermal insulation layer is in the shape of a rectangular plate, and the width of a single anti-crack thermal insulation layer is ≤1200mm, the height is ≤600mm, and the thickness is 50 to 100mm. The thickness of the anti-cracking and fireproof layer is 5mm to 8mm, and the thickness of the thermal insulation layer is 45mm to 72mm.
[0043] refer to Figure 3 The C-type ceramic spliced fireproof board 2 is formed by resin transfer molding with continuous fiber roving 23 to reinforce inorganic resin, and has good strength. In some specific embodiments, the continuous fiber roving 23 is at least one of basalt fiber, carbon fiber and glass fiber. The volume of the continuous fiber roving 23 accounts for 40% to 50% of the volume of the C-type ceramic spliced fireproof board 2. The inorganic resin is a ceramic geopolymer, and a commercial ceramic geopolymer matrix MEYEB can be used. As an example, the thickness of the C-type ceramic spliced fireproof board is 10 to 15 mm, and the lengths of the upper extension plate and the lower extension plate in the direction perpendicular to the C-type ceramic spliced fireproof board are not less than 20 mm.
[0044] refer to Figure 5 to Figure 7The inorganic shear connector 4 is composed of a connected screw part 41 and a nut part 42, and the inorganic shear connector 4 includes an embedded reinforcement layer 43 located inside and an outer insulation layer 44 wrapped around the outer periphery of the embedded reinforcement layer 43; the embedded reinforcement layer 43 is obtained by compression molding using mini FRP bars 45 to reinforce inorganic resin, which is used to improve the shear resistance of the inorganic shear connector and ensure that the inorganic shear connector can play an anchoring role; the outer insulation layer 44 is prepared by molding with foam-modified geopolymer, which is used to tie and limit the base wall outside the anti-cracking insulation layer, and at the same time ensure that the inorganic shear connector will not fail due to high temperature during a fire, thereby avoiding the separation of the base wall and the anti-cracking insulation layer. In some specific embodiments, the foam-modified geopolymer is a slurry obtained by stirring and mixing sodium silicate solution, low-calcium fly ash, foaming agent and water in a mass ratio of 8:7:(1.9-3.8):5. The foaming agent is any one of hollow glass microspheres, silica aerogel, and protein foaming agent. The mini FRP ribs 45 are at least one of BFRP ribs (basalt fiber), CFRP ribs (carbon fiber), and GFRP ribs (glass fiber). The length of the mini FRP ribs 45 is 10 mm smaller than the diameter of the screw portion 41, and the diameter of the mini FRP ribs 45 is 1 / 40 to 1 / 50 of the length of the mini FRP ribs 45. The mini FRP ribs 45 are arranged in three rows along the circumferential direction in the embedded reinforcement layer 43, and the spacing between each row of mini FRP ribs 45 is one-fourth of the diameter of the embedded reinforcement layer 43. The number of mini FRP ribs 45 in the outermost row is not less than 8, the number of mini FRP ribs 45 in the middle row is not less than 4, and the number of mini FRP ribs 45 in the innermost row is not less than 1. As an example, the length of the inorganic shear connector is the sum of the thickness of the crack-resistant insulation layer plus the anchoring depth of not less than 50 mm; the diameter of the screw portion is 25 to 40 mm; the diameter of the nut portion is not less than 50 mm, and the thickness of the nut portion is 1 / 4 to 1 / 2 of the diameter of the nut portion; the diameter of the embedded reinforcement layer is 20 to 35 mm; the thickness of the external insulation layer is 5 to 10 mm; the shear strength of the inorganic shear connector is not less than 50% of its tensile strength.
[0045] The base wall 1 is built with geopolymer mortar masonry bricks. In some specific embodiments, the preparation method of geopolymer mortar masonry bricks is: sodium silicate solution with a modulus of 2.3, S105 slag and quartz sand fine aggregate are uniformly stirred at a mass ratio of 1:1.25:1.5 using a mechanical stirrer under normal temperature-atmospheric environment for 5 minutes to obtain geopolymer mortar, and the obtained geopolymer mortar is injected into a masonry brick mold of a standard size, and after standard curing (20±2℃, 97%RH) for 28 days, geopolymer mortar masonry bricks are obtained. The compressive strength of geopolymer mortar masonry bricks is 33MPa. As an example, the thickness of the base wall 1 is 240mm. The side surface of the base wall 1 is provided with no less than 4 of the reserved channels 11 per square meter. The diameter of the reserved channel is 3mm larger than the diameter of the screw portion of the inorganic shear connector; the depth of the reserved channel is greater than 50mm.
[0046] The sealing inorganic glue 5 is a geopolymer slurry obtained by uniformly mechanically stirring a sodium silicate solution with a modulus of 2.3 and S105 slag at a mass ratio of 1:1.25 at room temperature. After 28 days of standard curing, the compressive strength is not less than 50 MPa.
[0047] The present invention is further described in detail below through detailed embodiments in conjunction with the accompanying drawings.
[0048] In the embodiments and comparative examples, the experimental methods used are conventional methods unless otherwise specified, and the materials, reagents, etc. used are all commercially available unless otherwise specified.
[0049] Example 1
[0050] refer to Figure 1 to Figure 7The present embodiment provides a prefabricated geopolymer wall that integrates thermal insulation, heat insulation, and dual fire protection, including a base wall 1, one side of the base wall 1 is connected to a C-type ceramic splicing fireproof board 2, and the other side of the base wall 1 is connected to an anti-cracking thermal insulation layer 3. The upper and lower ends of the C-type ceramic splicing fireproof board 2 are respectively provided with an upper extension plate 21 and a lower extension plate 22 that are clamped and fixed to the base wall 1. The anti-cracking thermal insulation layer 3 is connected to the base wall 1 through an inorganic shear connector 4. The base wall 1 is provided with a reserved channel 11 for riveting the inorganic shear connector 4 on the surface of one side facing the anti-cracking thermal insulation layer 3, and the pores between the reserved channel 11 and the inorganic shear connector 4 are filled with a sealed inorganic glue 5. Among them, the anti-cracking thermal insulation layer 3 includes an anti-cracking fireproof layer 31 and a thermal insulation layer 32. The thermal insulation layer 32 is prepared from foam-modified geopolymer. The anti-cracking fireproof layer 31 is prepared from inorganic resin mortar reinforced with a fiber woven mesh 33. The C-type ceramic splicing fireproof board 2 is formed by using continuous fiber roving 23 to reinforce inorganic resin through resin transfer molding. The inorganic shear connector 4 is composed of a connected screw part 41 and a nut part 42. The inorganic shear connector 4 includes an embedded reinforcement layer 43 located inside and an outer insulation layer 44 wrapped around the outer periphery of the embedded reinforcement layer 43; the embedded reinforcement layer 43 is obtained by using mini FRP bars 45 to reinforce inorganic resin through molding; the outer insulation layer 44 is prepared by using foam-modified geopolymer molding. The sealing inorganic glue 5 is a geopolymer slurry obtained by uniform mechanical stirring of a sodium silicate solution with a modulus of 2.3 and S105 slag at a mass ratio of 1:1.25 at room temperature. After 28 days of standard curing, the compressive strength is not less than 50MPa.
[0051] ① Setting of base wall
[0052] Geometric dimensions: The thickness of the base wall 1 is 240 mm, and the wall height is 3.3 m. No less than 4 reserved channels 11 are provided per square meter on the side surface of the base wall 1. The diameter of the reserved channel 11 is 3 mm larger than the diameter of the screw portion 41 of the inorganic shear connector 4; the depth of the reserved channel 11 is greater than 50 mm.
[0053] Material composition and preparation: The base wall 1 is built with geopolymer mortar masonry bricks. The preparation method of geopolymer mortar masonry bricks is as follows: Sodium silicate solution with a modulus of 2.3, S105 slag and quartz sand fine aggregate are uniformly stirred at a mass ratio of 1:1.25:1.5 using a mechanical stirrer at room temperature-atmospheric environment for 5 minutes to obtain geopolymer mortar, and the obtained geopolymer mortar is injected into a masonry brick mold of a standard size, and after standard curing (20±2℃, 97%RH) for 28 days, a geopolymer mortar masonry brick is obtained. The compressive strength of the geopolymer mortar masonry brick is 33MPa.
[0054] ②Setting of C-type ceramic splicing fireproof board
[0055] Geometric dimensions: The thickness of a single C-shaped ceramic spliced fireproof board 2 is 10 mm, the length is 3.305 m, the width is 1200 mm, and the length of the upper extension board 21 and the lower extension board 22 in the direction perpendicular to the C-shaped ceramic spliced fireproof board is 20 mm.
[0056] Material composition and preparation: Continuous fiber roving 23 uses 24000tex carbon fiber, and uses a positioning device to evenly arrange and fix the continuous fiber roving in a C-shaped steel mold. The volume of the continuous fiber roving accounts for 40% of the volume of the C-shaped ceramic spliced fireproof board. After the mold is closed, an inorganic resin (using a commercial ceramic geopolymer matrix MEYEB) is injected, and RTM technology (resin transfer molding) is used to cure at 80°C and 0.69MPa for 1 hour, and then at 250°C and 0.69MPa for 5 hours. After curing, demolding is completed. According to the test method of continuous fiber reinforced resin composite board, the continuous fiber roving and inorganic resin are prepared into an inorganic composite board with a length of 300mm, a width of 25mm, and a thickness of 0.2mm. The bending strength at room temperature is 285MPa. After being treated at 1000°C for 2 hours, the bending strength retention rate is 80%.
[0057] ③ Setting of anti-cracking insulation layer
[0058] Geometric dimensions: The anti-crack insulation layer 3 is in the shape of a rectangular plate, and the width of a single anti-crack insulation layer 3 is 1200 mm, the height is 600 mm, and the thickness is 50 mm. The thickness of the anti-crack fireproof layer 31 is 5 mm, and the thickness of the thermal insulation layer 32 is 45 mm.
[0059] Material composition and preparation:
[0060] (1) Preparation of thermal insulation layer: Sodium silicate solution with a modulus of 3.33, first-grade low-calcium fly ash, protein foaming agent and municipal tap water were mixed in a mass ratio of 8:7:2:5, and stirred at a high speed of not less than 500 rpm at room temperature to obtain a slurry. The slurry was then injected into a steel mold to the designed thickness of the thermal insulation layer, covered with a steel plate and sealed, and then cured at standard pressure and 45°C for 6 hours and at standard pressure and 100°C for 5 hours to form a thermal insulation layer with a compressive strength of 0.79 MPa and a thermal conductivity of 0.040 Wm -1 K -1 ;
[0061] (2) Preparation of anti-cracking and fireproof layer: remove the upper steel plate, roughen and sandblast the upper part of the thermal insulation layer; then install two layers of 24000tex carbon fiber woven mesh with a mesh size of 50mm*50mm in the middle of the 5mm thick mold (before use, acrylic resin is evenly coated on the surface and pressed and shaped using a flat plate), the spacing between the carbon fiber woven mesh is 2mm, and then inject inorganic resin (commercial ceramic geopolymer matrix MEYEB) and quartz sand in a mass ratio of 1:1.25 to obtain an inorganic resin mortar to the designed height of the anti-cracking and fireproof layer, close the mold again, cure at 80℃ and 0.69MPa for 1 hour, and then cure at 250℃ and 0.69MPa for 5 hours, and demold after curing.
[0062] The bending strength of the anti-cracking insulation layer at room temperature is 150MPa. After being treated at 1000°C for 2 hours, the bending strength retention rate is 82%.
[0063] ④ Setting of inorganic shear connectors
[0064] Geometric dimensions: The length of the inorganic shear connector 4 is 140 mm, the length of the screw portion 41 is 120 mm, the diameter of the screw portion 41 is 40 mm, the diameter of the nut portion 42 is 60 mm, the thickness of the nut portion 42 is 20 mm, the diameter of the embedded reinforcement layer 43 is 30 mm, and the thickness of the outer insulation layer 44 is 5 mm. The mini FRP ribs 45 are CFRP ribs (carbon fiber) with a length of 30 mm and a diameter of 0.6 mm. The mini FRP ribs are arranged in 3 rows along the circumferential direction in the embedded reinforcement layer, and the spacing between each row of mini FRP ribs is 7.5 mm. The number of mini FRP ribs in the outermost row is 8, the number of mini FRP ribs in the middle row is 4, and the number of mini FRP ribs in the innermost row is 1. The shear strength of the inorganic shear connector is not less than 50% of its tensile strength.
[0065] Material composition and preparation:
[0066] (1) Preparation of embedded reinforcement layer: The mini CFRP bars were installed in the steel mold of the internal reinforcement layer as required, and then an inorganic resin (commercial ceramic geopolymer matrix MEYEB) was injected into the mold. The RTM technology (resin transfer molding) was used to cure the steel bars at 80°C and 0.69 MPa for 1 hour, and then at 250°C and 0.69 MPa for 5 hours.
[0067] (2) Preparation of the outer insulation layer: After that, the steel mold for the outer insulation layer is installed, and the foam-modified geopolymer obtained by mixing a sodium silicate solution with a modulus of 3.33, a first-grade low-calcium fly ash, a protein foaming agent and water in a mass ratio of 8:7:2:5 is injected. After the mold is closed, it is cured at 0.5 MPa and 80°C for 6 hours and then removed from the mold.
[0068] The tensile strength and shear strength of the inorganic shear connector are 380MPa and 190MPa respectively.
[0069] Example 2
[0070] refer to Figure 1 to Figure 7 This embodiment provides a geopolymer prefabricated wall that integrates thermal insulation, heat insulation, and dual fire protection. The basic structure is similar to that of embodiment 1, except that:
[0071] ① The setting of the base wall is the same as that in Example 1, so it will not be repeated here.
[0072] ②Setting of C-type ceramic splicing fireproof board
[0073] Geometric dimensions: The thickness of a single C-shaped ceramic spliced fireproof board 2 is 15 mm, the length is 3.305 m, the width is 1000 mm, and the length of the upper extension board 21 and the lower extension board 22 in the direction perpendicular to the C-shaped ceramic spliced fireproof board is 22 mm.
[0074] Material composition and preparation: The continuous fiber roving 23 uses 24000tex basalt fiber, and the volume of the continuous fiber roving accounts for 47% of the volume of the C-type ceramic splicing fireproof board. The installation, curing process and sample testing method of the continuous fiber roving are the same as those in Example 1, so they are not repeated here. The bending strength of the C-type ceramic splicing fireproof board at room temperature is 190MPa, and after being treated at 1000℃ for 2 hours, the bending strength retention rate is 85%.
[0075] ③ Setting of anti-cracking insulation layer
[0076] Geometric dimensions: The anti-crack insulation layer 3 is in the shape of a rectangular plate, and the width of a single anti-crack insulation layer 3 is 1000 mm, the height is 500 mm, and the thickness is 55 mm. The thickness of the anti-crack fireproof layer 31 is 5.5 mm, and the thickness of the thermal insulation layer 32 is 49.5 mm.
[0077] Material composition and preparation:
[0078] (1) Preparation of thermal insulation layer: Sodium silicate solution with a modulus of 3.33, first-grade low-calcium fly ash, protein foaming agent and municipal tap water are mixed in a mass ratio of 8:7:3.5:5, and stirred at a high speed of not less than 500 rpm at room temperature to obtain a slurry. The slurry is then injected into a steel mold to the designed thickness of the thermal insulation layer, covered with a steel plate and sealed, and then cured at standard pressure and 45°C for 6 hours and at standard pressure and 100°C for 5 hours to form a thermal insulation layer with a compressive strength of 0.65 MPa and a thermal conductivity of 0.035 Wm -1 K -1 ;
[0079] (2) Preparation of anti-cracking fireproof layer: remove the upper steel plate, roughen and sandblast the upper part of the thermal insulation layer; then install two layers of 24000tex basalt fiber woven mesh with a mesh size of 25mm*25mm in the middle of the 5.5mm thick mold (before use, acrylic resin is evenly coated on the surface and shaped using a flat plate). The spacing between the basalt fiber woven meshes is 2.5mm, and the subsequent pouring and curing process is the same as in Example 1.
[0080] The flexural strength of the anti-cracking thermal insulation layer at room temperature is 130 MPa. After being treated at 1000°C for 2 hours, the flexural strength retention rate is 79%.
[0081] ④ Setting of inorganic shear connectors
[0082] Geometric dimensions: the length of the inorganic shear connector 4 is 140 mm, the length of the screw portion 41 is 115 mm, the diameter of the screw portion 41 is 35 mm, the diameter of the nut portion 42 is 55 mm, the thickness of the nut portion 42 is 25 mm, the diameter of the embedded reinforcement layer 43 is 30 mm, and the thickness of the outer insulation layer 44 is 2.5 mm. The configuration of the mini FRP rib 45 is the same as that of Example 1.
[0083] Material composition and preparation: The preparation of the embedded reinforcement layer and the outer insulation layer is the same as that in Example 1, so it will not be repeated here. The tensile strength and shear strength of the inorganic shear connector are 350 MPa and 175 MPa, respectively.
[0084] Example 3
[0085] refer to Figure 1 to Figure 7 This embodiment provides a geopolymer prefabricated wall that integrates thermal insulation, heat insulation, and dual fire protection. The basic structure is similar to that of embodiment 1, except that:
[0086] ① The setting of the base wall is the same as that in Example 1, so it will not be repeated here.
[0087] ②Setting of C-type ceramic splicing fireproof board
[0088] Geometric dimensions: The thickness of a single C-shaped ceramic spliced fireproof board 2 is 12 mm, the length is 3.305 m, the width is 900 mm, and the lengths of the upper extension board 21 and the lower extension board 22 in the direction perpendicular to the C-shaped ceramic spliced fireproof board are both 22 mm.
[0089] Material composition and preparation: The continuous fiber roving 23 uses 24000tex basalt fiber, and the volume of the continuous fiber roving accounts for 47% of the volume of the C-type ceramic splicing fireproof board. The installation, curing process and sample testing method of the continuous fiber roving are the same as those in Example 1, so they are not repeated here. The bending strength of the C-type ceramic splicing fireproof board at room temperature is 190MPa, and after being treated at 1000℃ for 2 hours, the bending strength retention rate is 85%.
[0090] ③ Setting of anti-cracking insulation layer
[0091] Geometric dimensions: The anti-crack insulation layer 3 is in the shape of a rectangular plate, and the width of a single anti-crack insulation layer 3 is 900 mm, the height is 450 mm, and the thickness is 80 mm. The thickness of the anti-crack fireproof layer 31 is 8 mm, and the thickness of the thermal insulation layer 32 is 72 mm.
[0092] Material composition and preparation:
[0093] (1) Preparation of thermal insulation layer: Sodium silicate solution with a modulus of 3.33, first-grade low-calcium fly ash, protein foaming agent and municipal tap water were mixed in a mass ratio of 8:7:2.6:5, and stirred at a high speed of not less than 500 rpm at room temperature to obtain a slurry. The slurry was then injected into a steel mold to the designed thickness of the thermal insulation layer, covered with a steel plate and sealed, and then cured at standard pressure and 45°C for 6 hours and at standard pressure and 100°C for 5 hours to form a thermal insulation layer with a compressive strength of 0.70 MPa and a thermal conductivity of 0.044 Wm -1 K -1 ;
[0094] (2) Preparation of anti-cracking fireproof layer: remove the upper steel plate, roughen and sandblast the upper part of the thermal insulation layer; then install three layers of 24000tex glass fiber woven mesh with a mesh size of 30mm*30mm in the middle of the 8mm thick mold (before use, acrylic resin is evenly coated on the surface and shaped using a flat plate). The spacing between the glass fiber woven meshes is 2mm, and the subsequent pouring and curing process is the same as in Example 1.
[0095] The bending strength of the anti-cracking insulation layer at room temperature is 120MPa. After being treated at 1000°C for 2 hours, the bending strength retention rate is 82%.
[0096] ④ Setting of inorganic shear connectors
[0097] Geometric dimensions: The length of the inorganic shear connector 4 is 165 mm, the length of the screw portion 41 is 140 mm, the diameter of the screw portion 41 is 40 mm, the diameter of the nut portion 42 is 70 mm, the thickness of the nut portion 42 is 25 mm, the diameter of the embedded reinforcement layer 43 is 33 mm, and the thickness of the outer insulation layer 44 is 3.5 mm. The spacing of each row of mini FRP ribs 45 is 8.25 mm, and the rest of the configuration of the mini FRP ribs 45 is the same as that of Example 1.
[0098] Material composition and preparation: The preparation of the embedded reinforcement layer and the outer insulation layer is the same as that in Example 1, so it will not be repeated here. The tensile strength and shear strength of the inorganic shear connector are 355 MPa and 180 MPa, respectively.
[0099] The above embodiments are merely illustrative of the concept and technical solution of the present invention, and are not intended to limit the present invention. Anyone familiar with the technology may modify or change the above embodiments without violating the spirit and scope of the present invention. Therefore, all equivalent modifications or changes made by a person with ordinary knowledge in the technical field without departing from the spirit and technical ideas disclosed by the present invention should still be covered by the claims of the present invention.
[0100] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This narrative method of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each implementation mode may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.
Claims
1. A geopolymer prefabricated wall with thermal insulation, heat insulation and double fire protection, including a base wall, characterized in that: One side of the base wall is connected to a C-shaped ceramic splicing fireproof board, and the other side of the base wall is connected to an anti-cracking thermal insulation layer; the upper and lower ends of the C-shaped ceramic splicing fireproof board are respectively provided with an upper extension plate and a lower extension plate which are clamped and fixed to the base wall, and the anti-cracking thermal insulation layer is connected to the base wall through an inorganic shear-resistant connector, and a reserved channel for riveting the inorganic shear-resistant connector is correspondingly provided on the surface of the base wall on one side facing the anti-cracking thermal insulation layer, and the gap between the reserved channel and the inorganic shear-resistant connector is filled with sealing inorganic glue.
2. The all-geopolymer prefabricated wall according to claim 1, characterized in that: The anti-cracking heat-insulating layer comprises an anti-cracking fireproof layer and a heat-insulating layer. The heat-insulating layer is prepared from foam-modified geopolymer, and the anti-cracking fireproof layer is prepared from fiber woven mesh reinforced inorganic resin mortar.
3. The all-geopolymer prefabricated wall according to claim 2, characterized in that: The inorganic resin mortar is formed by uniformly mixing inorganic resin and quartz sand in a mass ratio of 1:1.25; the fiber woven mesh is at least one of a basalt fiber woven mesh, a carbon fiber woven mesh, and a glass fiber woven mesh; the fiber woven mesh is evenly arranged in several layers, and the spacing between the fiber woven meshes is 1 to 3 mm.
4. The all-geopolymer prefabricated wall according to claim 1, characterized in that: The C-type ceramic spliced fireproof board is formed by using continuous fiber roving to reinforce inorganic resin through resin transfer molding; the continuous fiber roving is at least one of basalt fiber, carbon fiber and glass fiber; the volume of the continuous fiber roving accounts for 40% to 50% of the volume of the C-type ceramic spliced fireproof board.
5. The all-geopolymer prefabricated wall according to claim 3 or 4, characterized in that: The inorganic resin is a ceramic geopolymer.
6. The all-geopolymer prefabricated wall according to claim 1, characterized in that: The inorganic shear-resistant connector is composed of a connected screw part and a nut part, and includes an embedded reinforcement layer located inside and an outer insulation layer wrapped around the outer periphery of the embedded reinforcement layer; the embedded reinforcement layer is obtained by compression molding using mini FRP bars to reinforce inorganic resin; the outer insulation layer is prepared by molding using foam-modified geopolymer.
7. The all-geopolymer prefabricated wall according to claim 6, characterized in that: The mini FRP bars are at least one of BFRP bars, CFRP bars and GFRP bars; the length of the mini FRP bars is 10 mm smaller than the diameter of the screw portion, and the diameter of the mini FRP bars is 1 / 40 to 1 / 50 of the length of the mini FRP bars; the mini FRP bars are arranged in three rows along the circumferential direction in the embedded reinforcement layer, the spacing between the mini FRP bars in each row is one-fourth of the diameter of the embedded reinforcement layer, the number of mini FRP bars in the outermost row is not less than 8, the number of mini FRP bars in the middle row is not less than 4, and the number of mini FRP bars in the innermost row is not less than 1.
8. The all-geopolymer prefabricated wall according to claim 2 or 6, characterized in that: The foam-modified geopolymer is a slurry obtained by stirring and mixing sodium silicate solution, low-calcium fly ash, foaming agent and water in a mass ratio of 8:7:(1.9-3.8):5; the foaming agent is any one of hollow glass microspheres, silica aerogel and protein foaming agent.
9. The all-geopolymer prefabricated wall according to claim 1, characterized in that: The base wall is built with geopolymer mortar masonry bricks; and no less than 4 of the reserved channels are provided per square meter on the side surface of the base wall.
10. The all-geopolymer prefabricated wall according to claim 1, characterized in that: The sealing inorganic adhesive is a geopolymer slurry obtained by uniformly mechanically stirring a sodium silicate solution with a modulus of 2.3 and S105 slag in a mass ratio of 1:1.25 under normal temperature.