Method for measuring content of high-grade cadmium in lead smelting bottom blowing soot through microwave digestion-titration method

Through microwave digestion-titration method combined with zinc reference solution and EDTA standard solution, the problem of insufficient end point of cadmium determination in the soot blown ash in lead smelting bottom is solved, and the accurate determination of high-grade cadmium is achieved, which reduces cost and operational complexity. It is suitable for Detection of high cadmium content.

CN118980787APending Publication Date: 2024-11-19WESTERN MINING CO LTD +2

Patent Information

Application Number
CN202411083231.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art has problems such as insufficient titration end point and serious tailing when determining the high-grade cadmium content in lead smelting bottom blown ash, resulting in low accuracy of the measurement results, high cost and cumbersome operation, and is not suitable for batch sample testing.

Method used

By microwave digestion-titration, the pH was adjusted to 5.5-6 by adding zinc benchmark solution and EDTA standard solution to the volumetric flask, and combining with the dicresol orange indicator, the end point of the titration was obvious. , realize accurate measurement of cadmium.

Benefits of technology

It realizes accurate and rapid measurement of medium and high-grade cadmium in the lead smelting bottom blown ash, reduces detection costs, simplifies the operation process, improves the repetition and accuracy of the results, and is suitable for the detection of high-quality cadmium content.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118980787A_ABST
    Figure CN118980787A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of analytical chemistry, and particularly relates to a method for measuring the content of high-grade cadmium in lead smelting bottom blowing soot through a microwave digestion-titration method. The method comprises the following steps: (1) weighing a lead smelting bottom blowing soot sample, and digesting the sample through a microwave digestion method to obtain a sample solution; (2) transferring the sample solution to a volumetric flask, adding water, and fixing the volume to obtain a solution B; (3) transferring the zinc reference solution A and the solution B into a container, dropwise adding a xylenol orange indicator, adjusting the solution to be amaranth by using a hexamethylenetetramine buffer solution and enabling the solution to be excessive by 5mL, titrating by using an EDTA standard solution until the solution is changed from amaranth to luminous yellow, and recording the volume v of the EDTA standard solution consumed by titration; and (4) calculating the cadmium content according to a formula. According to the method, the zinc reference solution is added into the sample solution to be detected, the EDTA standard solution is used for titration, the titration end point is obviously jumped, accurate and rapid determination of cadmium is realized, the result is accurate and reliable, and the industry blank is filled.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of analytical chemistry, and in particular relates to a method for determining the high-grade cadmium content in bottom-blown ash from lead smelting by microwave digestion-titration. Background Art

[0002] There are many methods for the determination of cadmium, including graphite furnace atomic absorption spectrometry, electrochemical analysis, anodic stripping voltammetry, scanning polarography, colloidal gold immunochromatography, chemical colorimetry, inductively coupled plasma mass spectrometry, etc. Graphite furnace atomic absorption spectrometry is suitable for the determination of cadmium in various foods and soils. Electrochemical analysis methods include anodic stripping voltammetry and scanning polarography, which are suitable for the detection of heavy metal cadmium. Colloidal gold immunochromatography is suitable for the rapid detection of cadmium ions. In chemical colorimetry, cadmium ions in water samples react with dithizone in a strong alkaline solution and then are measured spectrophotometrically. According to different application scenarios and needs, you can choose a suitable determination method. For example, in the fields of environmental monitoring, food safety, and medical diagnosis, there are specific cadmium determination techniques and standards.

[0003] At present, the detection methods with reference value for cadmium detection mainly include atomic absorption spectrometry: GB / T8151.8-2012, detection range 0.10-2.00%; inductively coupled plasma emission spectrometry: GB / T8151.20-2012, detection range 0.050-2.00%; GB / T 3884.18-2023, detection range 0.003-0.40%; GB / T 12689.12-2004, detection range 0.0005-0.50%, etc., as well as X-ray fluorescence spectrometry, inductively coupled plasma mass spectrometry, dithizone extraction photometry, cadmium reagent spectrophotometry, etc. Spectrophotometry is the most commonly used method due to its simple instrumentation and low analysis cost. The above detection methods are all aimed at the determination of trace amounts of cadmium. For the determination of cadmium greater than 5%, YS / T 1512.7-2021 "Chemical Analysis Methods for Copper Smelting Dust - Determination of Cadmium Content - Flame Atomic Absorption Spectrometry and Titration" was found. This standard uses the back titration method for cadmium with a content of 5.00-17.00%. This method uses a 1g / L zinc standard solution for titration. Metallic zinc is expensive, the dosage is large, and the cost is high. In addition, data correction of filter residues must be done, the operation is cumbersome, the process is long, the result accuracy is low, and it is not suitable for batch sample testing. When this method is used to analyze cadmium in bottom-blown ash from lead smelting, due to differences in sample properties and impurities, the sample dissolution process splashes severely and the repeatability of the titration results is poor, so accurate results for cadmium cannot be obtained. No relevant testing basis was found for the determination of content greater than 17%. At the same time, copper smelting smoke and lead smelting bottom-blown ash belong to two smelting systems. The sample properties and impurities are very different. The YS / T 1512.7-2021 titration method is not applicable when determining the cadmium content in lead smelting bottom-blown ash.

[0004] The bottom-blown soot from lead smelting contains a lot of lead, cadmium and other valuable metals, with the lead content reaching 50% and the cadmium content reaching more than 20%. If it cannot be effectively enriched and recovered, it will cause a huge waste of associated resources. The invention patent with publication number CN102757023 A "Method for recovering selenium from lead smelting soot", the invention patent with publication number CN102757024 A "Method for recovering tellurium from lead smelting soot", and the Chinese patent with publication number CN 104263954B disclose "A method for comprehensive utilization of bottom-blown furnace soot from lead smelting", which can effectively recover and comprehensively utilize bottom-blown furnace soot. The study on how to recover non-ferrous metal resources was conducted from the perspective of chemical smelting technology, and it does not involve chemical analysis and detection technology. The invention patent with publication number CN 104263954 B discloses "A method for comprehensive recovery and utilization of lead-containing smoke generated in lead smelting", which can effectively recover and reuse 5% to 10% of zinc, about 20% of cadmium and about 40% of lead in the smoke of the bottom-blown furnace of lead smelting, and does not involve chemical analysis and detection technology.

[0005] The Chinese patent with publication number CN 103163118 B discloses the determination of trace cadmium in environmental samples by ICP method. The patent with publication number CN102478520 A "Determination of trace cadmium in zinc base" discloses the optimal determination conditions of trace cadmium in oil system by using fuzzy prediction technology in the presence of interference of a large amount of heavy metal ions such as copper, zinc and lead. The invention patent with publication number CN111458332 A "Method for determination of lead, zinc and cadmium from mixed lead-zinc-cadmium concentrate" adopts precipitation, masking, difference subtraction and other methods to solve the problem that the lead, zinc and cadmium content of the sample in the mixed lead-zinc-cadmium concentrate is greater than 4% and the lead, zinc and cadmium content are determined at the same time. The operation process of this method is cumbersome, time-consuming and not easy to master. Due to the difference in sample properties and impurities, this method has many technical defects and is not applicable when using lead smelting bottom blowing soot for experimental verification.

[0006] Zinc and cadmium belong to the same group of elements with similar chemical properties. To achieve the single determination of cadmium, zinc will cause serious interference and must be removed or masked. Potassium iodide and sodium pyrophosphate can be used to mask cadmium. The method of successfully masking zinc and accurately titrating cadmium has always been a common technical problem in the industry, and no suitable masking agent for zinc has been found. In addition, the determination of high-grade cadmium adopts the EDTA titration method. The color change during the titration process is slow and the tailing is serious. There is no obvious endpoint jump, and the accurate content of cadmium cannot be obtained. At present, there is no detection method for cadmium in cadmium concentrate. Therefore, it is of great value and application prospect to study the determination method of high-content cadmium, assist in the recovery of associated non-ferrous metal resources, improve the utilization rate of cadmium-containing resources, reduce resource waste, and generate economic benefits. Summary of the invention

[0007] The purpose of the present invention is to provide a method for determining the high-grade cadmium content in bottom-blown ash from lead smelting by microwave digestion-titration, which solves the problem of unclear endpoint jump and tailing in the direct titration method in the prior art. The method of the present invention is easy to master, has high accuracy, low cost, and is environmentally friendly, and is particularly suitable for accurately determining the cadmium content in bottom-blown ash from lead smelting containing more than 20% cadmium, 0.X% zinc, and 50% lead.

[0008] The implementation process of the present invention is as follows:

[0009] A method for determining the high-grade cadmium content in bottom-blown ash from lead smelting by microwave digestion-titration method comprises the following steps:

[0010] (1) Weighing a lead smelting bottom-blown ash sample, digesting the sample by microwave digestion to obtain a sample solution;

[0011] (2) Transfer the sample solution to a volumetric flask and add water to make up to volume to obtain solution B;

[0012] (3) The volume to be removed is v 1 The zinc standard solution A and volume v 2 Place solution B in a container, add xylenol orange indicator, adjust the solution to purple-red with hexamethylenetetramine buffer solution and add 5 mL excess, titrate with EDTA standard solution until the solution changes from purple-red to bright yellow, and record the volume v of EDTA standard solution consumed in the titration;

[0013] (4) Calculate the cadmium content according to the formula:

[0014]

[0015] Where:

[0016] w Cd ---Cadmium content, %;

[0017] c---Concentration of EDTA standard solution, mol / L;

[0018] c 1 ---Concentration of zinc standard solution, mg / mL;

[0019] c 2 ---The concentration of zinc in the sample solution was measured by flame atomic absorption spectrophotometry, ug / mL;

[0020] m---mass of the sample, g;

[0021] M 1 ---The molar mass of cadmium is 112.4 g / moL;

[0022] M 2 ---The molar mass of zinc is 65.38 g / moL;

[0023] v---the volume of EDTA standard solution consumed in titration, mL;

[0024] v 1 --- Volume of zinc standard solution A taken, mL;

[0025] v 2 ---Fixed volume of sample solution, mL.

[0026] Furthermore, the solvent of the microwave digestion method in step (1) is a mixture of aqua regia and sulfuric acid.

[0027] Furthermore, the concentration of zinc standard solution A in step (3) is 5 mg / mL.

[0028] Furthermore, the preparation process of zinc standard solution A is to accurately weigh 0.5000g of zinc ingot into a 400mL beaker, add 5mL of hydrochloric acid, dissolve it completely, transfer it to a 100mL volumetric flask after cooling, add water to make up the volume, and shake it well.

[0029] Furthermore, in step (3), when the hexamethylenetetramine buffer solution is adjusted to purple-red and an excess of 5 mL is added, the pH is 5.5-6.

[0030] Further, the concentration of zinc in solution B was measured by flame atomic absorption spectrophotometry according to GB / T 14353.3-2010 as c 2 .

[0031] Furthermore, in step (3), the preparation process of the xylenol orange indicator is as follows: weigh 1 g of the xylenol orange indicator into a 200 mL beaker, add 100 mL of water, dissolve it completely, add 2 drops of ammonia water to make the solution dark purple, and mix well.

[0032] Furthermore, in step (3), the mass percentage of the hexamethylenetetramine solution is 20%.

[0033] Furthermore, in step (3), the preparation process of the EDTA standard solution is to weigh 186g of disodium ethylenediaminetetraacetate into a 2L beaker, add water to dissolve it completely, heat it at low temperature until the solution is clear, filter it with absorbent cotton into a 20L bottom-mouthed bottle after cooling, add water to 20L, shake it well, and calibrate it after leaving it for one week.

[0034] Further, the calibration process of the EDTA standard solution is to accurately weigh 0.0500g of standard zinc oxide in a 500mL conical beaker, moisten with water, add 2mL of hydrochloric acid to dissolve completely, add 50mL of water, add 1 drop of methyl orange indicator, neutralize with ammonia water and hydrochloric acid until the solution changes from red to orange-yellow, rinse the wall of the cup with water, add 20mL of acetic acid-sodium acetate buffer solution and 1 drop of xylenol orange indicator, and titrate with EDTA standard solution until the solution changes from purple-red to bright yellow as the end point; perform parallel determination 3 times, and record the volume of the standard solution consumed (V 1 ), calculate the concentration c of the EDTA standard solution.

[0035] Compared with the prior art, the present invention has the following positive effects:

[0036] (1) Aiming at the characteristics of samples containing high lead, high cadmium and trace zinc in bottom-blown ash from lead smelting, a direct titration method was developed, which has low detection cost, friendly experimental environment, easy method mastering, good result reproducibility, and can accurately determine the high-grade cadmium in bottom-blown ash from lead smelting.

[0037] (2) The method of the present invention adds a certain amount of zinc reference solution to the sample solution to be tested, and uses EDTA standard solution for titration. The titration endpoint has an obvious jump, which realizes the accurate and rapid determination of cadmium. The result is accurate and reliable. It is a method for promoting the jump of cadmium titration endpoint, filling the gap in the industry.

[0038] (3) In the method of the present invention, high content of lead generates lead sulfate precipitate, which is slightly soluble in water and does not interfere with the determination.

[0039] (4) In step (3) of the method of the present invention, after the solution is adjusted to purple-red with 20% by mass hexamethylenetetramine buffer solution, an excess of 5 mL is required to maintain the pH at 5.5-6. The titration endpoint is bright yellow with an obvious jump, which can more accurately determine the titration endpoint. BRIEF DESCRIPTION OF THE DRAWINGS

[0040] Figure 1 This is a diagram of color change during the titration process of Example 1;

[0041] Figure 2 This is a diagram of color change during the titration process of Comparative Example 1;

[0042] Figure 3 It is a comparison chart of the titration endpoint colors of Example 1 and Comparative Example 1. DETAILED DESCRIPTION

[0043] The present invention will be further described below in conjunction with the embodiments.

[0044] The method of the present invention studies the re-dissolution system, the sample is completely dissolved, and the high-pressure microwave closed digestion technology is used for sample pretreatment, the microwave digestion technical parameters are determined, and the zinc standard is used in coordination to determine the accurate value of the zinc standard coordination, so as to achieve accurate determination of cadmium, and the endpoint jump is obvious. The method of the present invention introduces a dilution factor, reduces the amount of zinc standard, greatly reduces the detection cost, has high detection timeliness, and accurate results. The method of the present invention is suitable for the accurate determination of cadmium content in bottom-blown soot containing 0.X% zinc, 50% lead, and more than 20% cadmium. The method is simple, easy to master, highly accurate, highly time-effective, low detection cost, and obvious endpoint jump, filling the gap in the industry.

[0045] Example 1

[0046] (I) Reagents

[0047] Hydrochloric acid and nitric acid were of analytical grade;

[0048] Hexamethylenetetramine solution: mass percentage is 20%;

[0049] Xylenol orange indicator: weigh 1g of xylenol orange indicator into a 200mL beaker, add 100mL of water, dissolve completely, add 2 drops of ammonia water to make the solution dark purple, and mix well.

[0050] Methyl orange indicator: mass percentage is 0.05%;

[0051] Acetic acid-sodium acetate buffer solution: pH = 5.5-6.0;

[0052] Zinc ingot: mass percentage is 99.99%;

[0053] Zinc oxide: reference substance, mass percentage is 99.99%.

[0054] (II) Preparation and calibration of standard solutions

[0055] 1. Disodium ethylenediaminetetraacetate (Na 2 Preparation of EDTA standard solution (C≈0.025mol / L):

[0056] Weigh 186g of disodium ethylenediaminetetraacetate into a 2L beaker, add water to dissolve completely, heat at low temperature until the solution is clear, cool and filter with absorbent cotton into a 20L bottom-mouthed bottle, add water to 20L, shake well, and calibrate after leaving for one week.

[0057] 2. Standardization of disodium ethylenediaminetetraacetate standard solution:

[0058] Accurately weigh 0.0500g of standard zinc oxide in a 500mL conical beaker, moisten with a small amount of water, add 2mL of hydrochloric acid to dissolve completely, add 50mL of water, add 1 drop of methyl orange indicator, neutralize with ammonia water and hydrochloric acid until the solution changes from red to orange-yellow, rinse the wall of the cup with a small amount of water, add 20mL of acetic acid-sodium acetate buffer solution and 1 drop of xylenol orange indicator, and titrate with EDTA standard solution until the solution changes from purple-red to bright yellow as the end point. Repeat the measurement 3 times and record the volume of standard solution consumed (V 1 ), calculate the concentration c of the EDTA standard solution.

[0059] Blank test: do not add 0.05 g of reference zinc oxide, and the other steps are the same as above "2. Calibration of disodium ethylenediaminetetraacetic acid standard solution".

[0060] 3. Calculation of EDTA standard titration solution:

[0061]

[0062] Where: c---the concentration of EDTA standard solution, mol / L;

[0063] m 1 ---Mass of reference zinc oxide, g;

[0064] M 1 --- Molar mass of reference zinc oxide, 81.38 g / moL;

[0065] V 1 ---The volume of EDTA standard solution consumed for calibration, mL;

[0066] V 0 ---The volume of EDTA standard solution consumed in the blank test, mL.

[0067] 4. Zinc standard solution A (C 1 =5mg / mL): Accurately weigh 0.5000g zinc ingot into a 400mL beaker, add 5mL hydrochloric acid, dissolve completely, cool and transfer to a 100mL volumetric flask with a little water, make up to volume and shake well.

[0068] (III) Experimental process

[0069] (1) Accurately weigh 0.5000 g of 1# lead smelting bottom-blown fly ash sample (containing Pb: 49.55%) on a 50*50 mm weighing paper, pinch the weighing paper containing the sample into a small ball, place it in a digestion tank, add 8 mL of aqua regia and 2 mL of sulfuric acid, cover with a sealing lid, place it in a microwave digestion instrument, and digest the sample according to the microwave digestion heating program in Table 1.

[0070] Table 1 Microwave digestion heating program

[0071]

[0072]

[0073] (2) Transfer the sample digested and cooled in step (1) to a 100 mL volumetric flask, add water to make up to volume, and shake well to obtain solution B.

[0074] (3) Accurately pipette 5.00 mL (v 1 ) Zinc standard solution A and 20.00mL (v 2 ) Solution B was placed in the same 400mL beaker, 1 drop of xylenol orange indicator was added, the solution was adjusted to purple-red with 20% by mass hexamethylenetetramine buffer solution, and an excess of 5mL (pH 5.5-6) ​​was added, and the EDTA standard solution was titrated until the solution changed from purple-red to bright yellow. Figure 1 , record the volume v of EDTA standard solution consumed in titration.

[0075] (4) According to GB / T 14353.3-2010 flame atomic absorption spectrophotometry, the concentration of zinc in solution B is c 2 .

[0076] (5) Calculate the cadmium content according to the formula w Cd :

[0077]

[0078] Where:

[0079] w Cd ---Cadmium content, %;

[0080] c---Concentration of EDTA standard solution, mol / L;

[0081] c 1 ---Concentration of zinc standard solution, mg / mL;

[0082] c 2 ---The concentration of zinc in the sample solution was measured by flame atomic absorption spectrophotometry, ug / mL;

[0083] m---mass of the sample, g;

[0084] M 1 ---The molar mass of cadmium is 112.4 g / moL;

[0085] M 2 ---The molar mass of zinc is 65.38 g / moL;

[0086] v---the volume of EDTA standard solution consumed in titration, mL;

[0087] v 1 --- Take the volume of zinc standard solution A, mL.

[0088] v 2 ---Fixed volume of sample solution, mL.

[0089] The experimental results are shown in the following table:

[0090] Table 2 Experimental results of Example 1

[0091]

[0092]

[0093] Comparative Example 1:

[0094] The experimental process and parameters of this comparative example 1 are the same as those of Example 1, except that: in step (3), after adjusting the solution to purple-red with a 20% by mass hexamethylenetetramine buffer solution, no excess 5 mL of hexamethylenetetramine buffer solution was added; the color change during the titration process was Figure 2 .

[0095] Table 3 Experimental results of Example 1

[0096]

[0097] From the figures and data of Example 1 and Comparative Example 1, it can be seen that: (1) The color difference of the titration endpoint is that the color of the titration endpoint of the method of the present invention is completely different from the color of the titration process, see Figure 1-Figure 3 , which is conducive to accurate judgment of the titration endpoint, while the titration endpoint color and the titration process color of comparative example 1 are both close to orange, resulting in an unclear titration endpoint jump; (2) The measured Cd content fluctuates more than that of the method of the present invention, the maximum and minimum values ​​of the measurement result differ by 0.38%, and the average value of the measurement result differs by 0.19% from the instrumental measurement result.

[0098] Example 2

[0099] According to the method described in Example 1, the 2# lead smelting bottom-blown soot sample (containing Pb: 53.20%) was titrated.

[0100] The experimental results are shown in the following table:

[0101] Table 4 Experimental results of Example 1

[0102]

[0103] From the data of Example 1 and Example 2, it can be seen that the determination of Cd content by the method of the present invention does not affect the determination of Zn content, and the sample solution B can directly measure the zinc content by flame atomic absorption spectrophotometry. The average value of Cd content determined by the method of the present invention is closer to the result of instrumental determination, and the Cd content determined multiple times by the method of the present invention has good repeatability, small error, good data stability and high accuracy.

[0104] Compared with the prior art, the advantages of the present invention are:

[0105] (1) When the high-grade cadmium in lead smelting bottom-blown ash was determined by the method YS / T 1512.7-2021 "Chemical analysis method for copper smelting smoke - Determination of cadmium content", during the operation of step 5.5.4.1 "low-temperature heating until the hydrobromic acid is completely volatilized", the sample was severely splashed, resulting in sample loss and unstable measurement results: the difference between the maximum and minimum values ​​of the measurement results reached 0.72% for sample 1# and 0.75% for sample 2#, and the average value of the measurement results was significantly different from the instrumental measurement results, reaching 0.56% for sample 1# and 0.42% for sample 2#.

[0106] The sample dissolution of the method of the present invention is complete and easy to control without loss. The difference between the maximum value and the minimum value of the measurement result is 0.22% for sample 1# and 0.12% for sample 2#. The difference between the average value of the measurement result and the instrument measurement result is 0.17% for sample 1# and 0.14% for sample 2#. The accuracy of the detection result is much higher than that of the YS / T1512.7-2021 method. The method of the present invention is more accurate and stable for detecting high-content cadmium in bottom-blown ash from lead smelting.

[0107] (2) Perchloric acid and hydrobromic acid in the YS / T 1512.7-2021 method are expensive and easy to make poisons.

[0108] The method of the present invention does not require the above reagents, is environmentally friendly and beneficial to health.

[0109] (3) Compared with the YS / T 1512.7-2021 method, the method of the present invention saves about 80 mg of zinc per sample, and the cost is low.

[0110] (4) When using this method, the operation is simple and the process is short. For example, a batch of 10 samples can be tested in just 3 hours.

[0111] The YS / T 1512.7-2021 method requires at least 12 hours to complete.

[0112] (5) The YS / T 1512.7-2021 method requires filtration and precipitation, has a long operation process, and the precipitation requires a correction experiment, which is time-consuming, cumbersome, and has low accuracy.

[0113] The method of the invention is simple and rapid to operate, and has high accuracy and good precision.

[0114] (6) The YS / T 1512.7-2021 method is for copper smelting dust, with copper grade up to 20%, cadmium grade 5%-17%, lead grade 10%, and zinc grade 1%.

[0115] The method of the present invention is used for bottom-blown ash from lead smelting. The samples have different properties, with lead grade up to 50%, cadmium grade up to 30%, zinc grade 0.X%, and copper content less than 0.10%. Copper basically does not affect the determination.

[0116] (7) YS / T 1512.7-2021 method step 5.5.4.6 "Determine the pH value of the solution using a pH meter" The solution needs to use a pH meter to strictly control the acidity conditions.

[0117] The method of the present invention only requires 5 ml of excess buffer solution to reach the required pH value, and the operation is simple.

[0118] (8) The YS / T 1512.7-2021 method is for copper smelting dust, which has a high copper content.

[0119] The method of the present invention is aimed at the bottom-blown fly ash from lead smelting with high lead content and no copper. The properties of the samples are different, and the specific implementation steps of the YS / T 1512.7-2021 method cannot be fully adopted.

[0120] (9) The method of the present invention is mainly suitable for direct and accurate titration of cadmium with a grade greater than 20%, zinc with a grade of 0.X%, and lead with a grade of 50%. The YS / T 1512.7-2021 method uses a back titration method with a different principle. Different samples can achieve different results.

[0121] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and the specific implementation of the present invention cannot be limited to these descriptions. For ordinary technicians in the field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.

Claims

1. A method for determining the high-grade cadmium content in bottom-blown ash from lead smelting by microwave digestion-titration. It is characterized in that The steps include: (1) Weighing a lead smelting bottom-blown ash sample, digesting the sample by microwave digestion to obtain a sample solution; (2) Transfer the sample solution to a volumetric flask and add water to make up to volume to obtain solution B; (3) The volume to be removed is v 1 The zinc standard solution A and volume v 2 Place solution B in a container, add xylenol orange indicator, adjust the solution to purple-red with hexamethylenetetramine buffer solution and add 5 mL excess, titrate with EDTA standard solution until the solution changes from purple-red to bright yellow, and record the volume v of EDTA standard solution consumed in the titration; (4) Calculate the cadmium content according to the formula: Where: w Cd ---Cadmium content, %; c---Concentration of EDTA standard solution, mol / L; c 1 ---Concentration of zinc standard solution, mg / mL; c 2 ---The concentration of zinc in the sample solution was measured by flame atomic absorption spectrophotometry, ug / mL; m---mass of the sample, g; M 1 ---The molar mass of cadmium is 112.4 g / moL; M 2 ---The molar mass of zinc is 65.38 g / moL; v---the volume of EDTA standard solution consumed in titration, mL; v 1 ---Volume of zinc standard solution A taken, mL; v 2 ---Fixed volume of sample solution, mL.

2. The method according to claim 1, Features: The solvent of the microwave digestion method in step (1) is a mixture of aqua regia and sulfuric acid.

3. The method according to claim 1, Features: The concentration of zinc reference solution A in step (3) is 5 mg / mL.

4. The method according to claim 3, Features: The preparation process of zinc standard solution A is to accurately weigh 0.5000g of zinc ingot into a 400mL beaker, add 5mL of hydrochloric acid, dissolve it completely, transfer it to a 100mL volumetric flask after cooling, add water to make up the volume, and shake well.

5. The method according to claim 1, Features: In step (3), when the hexamethylenetetramine buffer solution is adjusted to purple-red and an excess of 5 mL is added, the pH is 5.5-6.

6. The method according to claim 1, Features: According to GB / T 14353.3-2010 flame atomic absorption spectrophotometry, the concentration of zinc in solution B is c 2 .

7. The method according to claim 1, Features: In step (3), the preparation process of xylenol orange indicator is as follows: weigh 1 g of xylenol orange indicator into a 200 mL beaker, add 100 mL of water, dissolve it completely, add 2 drops of ammonia water to make the solution dark purple, and mix well.

8. The method according to claim 1, Features: In step (3), the mass percentage of the hexamethylenetetramine solution is 20%.

9. The method according to claim 1, Features: In step (3), the preparation process of the EDTA standard solution is to weigh 186g of disodium ethylenediaminetetraacetate into a 2L beaker, add water to dissolve it completely, heat it at low temperature until the solution is clear, filter it with absorbent cotton into a 20L bottom-mouthed bottle after cooling, add water to 20L, shake it well, and calibrate it after leaving it for one week.

10. The method according to claim 9, Features: The calibration process of EDTA standard solution is to accurately weigh 0.0500g of standard zinc oxide in a 500mL conical beaker, moisten it with water, add 2mL of hydrochloric acid to dissolve it completely, add 50mL of water, add 1 drop of methyl orange indicator, neutralize it with ammonia water and hydrochloric acid until the solution changes from red to orange-yellow, rinse the wall of the cup with water, add 20mL of acetic acid-sodium acetate buffer solution and 1 drop of xylenol orange indicator, and titrate it with EDTA standard solution until the solution changes from purple-red to bright yellow as the end point; perform parallel determination 3 times and record the volume of standard solution consumed (V 1 ), calculate the concentration c of the EDTA standard solution.

Citation Information

Patent Citations

  • Method for determining cadmium heavy metal ion in oil liquid

    CN102478520A

  • Method for recovering selenium from lead smelting soot

    CN102757023A

  • Method for recovering tellurium from zinc ash from lead metallurgy

    CN102757024A

  • Method for measuring cadmium content in the environment using ICP method

    CN103163118B

  • A method for comprehensive utilization of flue dust in bottom blowing furnace of lead smelting

    CN104263954B

Cited By

  • Composite indicator for measuring content of cadmium in crude cadmium and testing method