Preparation method and application of microstructure polarizer

The broad-spectrum full Stokes microarray polarizer was prepared by photo-controlled orientation technology based on interlayer molecules self-organization, which solved the problem of insufficient contrast and clarity of polarization imaging technology in the existing technology, and achieved high performance and broad-spectrum Polarization imaging adapts to the simultaneous acquisition and wide application of multi-objective information.

CN118981072AActive Publication Date: 2024-11-19HUNAN UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411046114.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-31
Publication Date
2024-11-19
Estimated Expiration
2044-07-31

AI Technical Summary

Technical Problem

Most existing polarization imaging technologies are limited to single spectrum or infrared spectrum, resulting in insufficient image contrast and clarity, and are fragile in extreme environments, making it difficult to adapt to the simultaneous acquisition and wide application of multi-objective information.

Method used

Using photo-controlled orientation technology based on interlayer molecules, a broad-spectrum full Stokes microarray polarizer based on azo dye is prepared, and dye molecules are oriented using layered coating technology to form high-performance, broad-spectrum microstructures. Polarized plate.

Benefits of technology

It realizes high-performance, broad-spectrum polarization imaging, overcomes the narrow wavelength range and high cost problems of traditional polarization cameras, improves the robustness and stability of the system, and is suitable for a wider application environment.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118981072A_ABST
    Figure CN118981072A_ABST
Patent Text Reader

Abstract

The invention provides a preparation method and application of a microstructure polaroid, and the method comprises the steps: firstly preparing an orientation solution, then carrying out the spin coating of the orientation solution on a cleaned substrate, forming an outgoing layer, and then irradiating the orientation layer through linear polarization ultraviolet light, thereby obtaining a structured polarization orientation orientation layer with a programmable pattern. The method comprises the following steps: preparing a liquid crystal polymer solution, spin-coating the liquid crystal polymer solution on a pattern programmable structured polarization orientation layer to prepare a liquid crystal polymer monomer coating film, treating the liquid crystal polymer monomer coating film by using a photocuring process to obtain a liquid crystal polymer film, and depositing a polarization light-absorbing dye on the liquid crystal polymer film to form a polarization light-absorbing dye coating film. And obtaining the microstructure polaroid. According to the invention, challenges on stability and solubility when the dye and the liquid crystal molecules are mixed are avoided, and the stability of the optical thin film and the robustness of the system can be obviously improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of optical imaging and micro-nano optics, and particularly relates to a preparation method and application of a microstructured polarizer. Background Art

[0002] Polarization, as a fundamental property of light, plays a vital role in the field of optics and related technologies. Polarization imaging technology can reveal information that cannot be detected by conventional intensity cameras, such as the vector distribution of structured beams, the texture and stress of reflecting or transmitting surfaces, and the optical activity of biological materials. This technology has been widely used in many fields such as target recognition, seabed observation, biomedicine, ecological monitoring and stereoscopic vision enhancement, and has greatly promoted the understanding of the environment and the progress of scientific research. At the same time, it has also achieved breakthroughs in practical applications in many fields such as industry, medicine and environmental protection.

[0003] However, most of the existing polarization imaging technologies are limited to a single spectral band or infrared spectral band, and rely on narrow-band imaging methods, which limits the simultaneous acquisition of multi-target information and often leads to insufficient image contrast and clarity. In addition, these imaging systems are fragile under extremely harsh environmental conditions, and their applicability is limited to specific occasions. By integrating the spectral, polarization and spatial multi-dimensional data of the target, the development of polarization imaging technology is expected to significantly enhance the efficiency of target detection and recognition, and adapt to a wider range of application environments. Therefore, it is particularly important to develop polarization imaging systems that can cover a wider band, have excellent performance, high integration and high cost-effectiveness.

[0004] The split-focus plane polarization imaging devices currently on the market use micro-array polarizers as core components. They are outstanding for their compact structure and have been successfully commercialized. For example, the PolarCam CCD polarization camera launched by 4D Tech and the IMX250MZR CMOS polarization sensor of Sony represent the latest progress in this technology. The sub-wavelength metal wire grid micro-arrays used in these devices are constructed through specific preparation technologies such as electron beam lithography, nanoimprinting and laser interferometry. Although they have many advantages, they also have problems such as narrow working wavelength range, high cost and easy parameter variation during the manufacturing process.

[0005] To solve these problems, it is crucial to develop new materials and technologies, such as dyes with adjustable spectral absorption properties and optical devices based on micro-nano light-controlled orientation technology. These advances not only improve the flexibility and accuracy of polarization imaging, but also help promote the development of high-performance display. In summary, continuous optimization and innovation of polarization imaging technology are of great significance to meet the increasingly diverse application needs and improve the adaptability of operating environments. Summary of the invention

[0006] In view of the above situation, the main purpose of the present invention is to provide a preparation method and application of a microstructured polarizer to solve the above technical problems.

[0007] The present invention provides a method for preparing a microstructured polarizer, which is used to prepare the above-mentioned microstructured polarizer, and the method comprises the following steps:

[0008] Step 1: ultrasonically clean a substrate coated with an antireflection film on one side using an aqueous solution of an optical cleaning agent for a first preset time, then clean the aqueous solution of the optical cleaning agent on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at a first preset temperature for drying;

[0009] Step 2, dissolving the polarized light absorbing dye in dimethylformamide at a preset weight ratio to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then placing the substrate on a test bench at a second preset temperature and heating it for a second preset time to form an alignment layer;

[0010] Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation;

[0011] Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 and dissolving them in a toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating;

[0012] Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film;

[0013] Step 6: depositing a polarized light absorbing dye on the liquid crystal polymer film to form a polarized light absorbing dye coating to obtain a microstructured polarizer.

[0014] Furthermore, in step 1, the effective wavelength band of the antireflection film is 400-700 nm, and the first preset time is 15-20 min.

[0015] Furthermore, in step 1, the first preset temperature is 50-200°C.

[0016] Furthermore, in step 2, the weight ratio of the polarized light absorbing dye to dimethylformamide is 0.5 wt %.

[0017] Furthermore, in step 2, the second preset temperature is 50-200° C., and the second preset time is 1-60 min.

[0018] Furthermore, in step 4, the mixing mass ratio of the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 is 96:4.

[0019] Furthermore, in step 4, the mass percentage of the mixture of the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 and the toluene solvent is 15 wt %.

[0020] Furthermore, in step 6, the polarized light absorbing dye uses a mixed solvent of one or more of AD1, sudan III and sudan b1ack.

[0021] An application of a microstructured polarizer is a microstructured polarizer based on a light-controlled orientation technology prepared by the above-mentioned preparation method, wherein the microstructured polarizer based on the light-controlled orientation technology is used to capture polarization information of light.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The present invention proposes a light-controlled orientation technology based on interlayer molecular self-organization to prepare azo dye-based broad-spectrum full-Stokes microarray polarizers. This new method not only overcomes the main defects of traditional polarization cameras, but also is expected to effectively replace high-cost imported polarization cameras through more economical technical means.

[0024] 2. The self-organization technology based on layered coating adopted by the present invention can orient a wider range of dye molecules, which not only breaks the limitation of only a few azo dye molecules, but also significantly expands the range of material selection, thereby increasing the possibility of preparing high-performance, broad-spectrum full-Stokes microstructure polarizers. In addition, this technology avoids the stability and solubility challenges when dyes are mixed with liquid crystal molecules, which can significantly improve the stability of optical films and the robustness of the system.

[0025] Additional aspects and advantages of the present invention will be given in part in the following description and in part will be obvious from the following description or learned through embodiments of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a schematic diagram of the steps for preparing a microstructured polarizer;

[0027] Figure 2 It is the molecular structure diagram of three polarized light absorbing dyes;

[0028] Figure 3 This is a graph of the extinction ratio of the polarizer with AD11 as the dye versus wavelength;

[0029] Figure 4 This is a schematic diagram of the extinction ratio test optical path device;

[0030] Figure 5 Schematic diagram of the extinction ratio of AD1 polarizers prepared with different numbers of layers;

[0031] Figure 6 It is a schematic diagram of the exposure optical path of the laser direct writing system;

[0032] Figure 7 is a micrograph of an 8 μm × 8 μm dye microarray with transmission axes of 0° and 90°, prepared by laser direct writing method;

[0033] Figure 8 It is the average transmittance of the unidirectional sample prepared by laser direct writing exposure technology at 450nm and the schematic diagram of its fitting curve;

[0034] Fig. 9 is the patterned AD1 image on the flexible liquid crystal polymer film and the normalized extinction ratio of the flexible polarizer versus the number of bending cycles with a radius of 1 mm;

[0035] Fig.10 This is a graph showing the extinction ratio of a polarizer made with Sudan III as a polarization absorbing dye versus wavelength;

[0036] Fig.11 This is a graph showing the extinction ratio of a polarizer made with Sudan black as a polarization absorbing dye versus wavelength;

[0037] Fig.12 This is a curve of the extinction ratio of the polarizer made with AD1, sudan III, and sudan black mixed dyes as polarization absorbing dyes. DETAILED DESCRIPTION

[0038] Embodiments of the present invention are described in detail below, examples of which are shown in the accompanying drawings, wherein the same or similar reference numerals throughout represent the same or similar elements or elements having the same or similar functions. The embodiments described below with reference to the accompanying drawings are exemplary and are only used to explain the present invention, and cannot be understood as limiting the present invention.

[0039] These and other aspects of the embodiments of the present invention will be apparent with reference to the following description and accompanying drawings. In these descriptions and accompanying drawings, some specific implementations of the embodiments of the present invention are specifically disclosed to represent some ways of implementing the principles of the embodiments of the present invention, but it should be understood that the scope of the embodiments of the present invention is not limited thereto.

[0040] Example 1

[0041] An embodiment of the present invention provides a method for preparing a microstructure polarizer, the method is used to prepare the above-mentioned microstructure polarizer based on the light-controlled orientation technology, and the method comprises the following steps:

[0042] Step 1: ultrasonically clean a substrate coated with an anti-reflection film with an effective wavelength of 400 nm on one side using a 5% optical cleaning agent aqueous solution for 15 minutes, then clean the optical cleaning agent aqueous solution on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at 130° C. for drying;

[0043] Step 2, dissolving AD1 in dimethylformamide at 0.5 wt % to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then placing the substrate on a test bench at 100° C. and heating it for 5 min to form an alignment layer;

[0044] Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation;

[0045] Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 at a mass ratio of 96:4 and dissolving them in a 15wt% toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern-programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating;

[0046] Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film;

[0047] Step 6: AD1 is used as a polarized light-absorbing dye to be deposited on the liquid crystal polymer film to form a polarized light-absorbing dye coating to obtain a microstructured polarizer.

[0048] Example 2

[0049] An embodiment of the present invention provides a method for preparing a microstructure polarizer, the method is used to prepare the above-mentioned microstructure polarizer based on the light-controlled orientation technology, and the method comprises the following steps:

[0050] Step 1: ultrasonically clean a substrate coated with an anti-reflection film with an effective wavelength of 400 nm on one side using a 5% optical cleaning agent aqueous solution for 15 minutes, then clean the optical cleaning agent aqueous solution on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at 130° C. for drying;

[0051] Step 2, dissolving Sudan III in dimethylformamide at 0.5 wt % to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then placing the substrate on a test bench at 100° C. and heating it for 5 min to form an alignment layer;

[0052] Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation;

[0053] Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG1 84 at a mass ratio of 96:4 and dissolving them in a 15wt% toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern-programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating;

[0054] Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film;

[0055] Step 6: Using Sudan III as a polarized light-absorbing dye to deposit on the liquid crystal polymer film to form a polarized light-absorbing dye coating to obtain a microstructured polarizer.

[0056] Example 3

[0057] An embodiment of the present invention provides a method for preparing a microstructure polarizer, the method is used to prepare the above-mentioned microstructure polarizer based on the light-controlled orientation technology, and the method comprises the following steps:

[0058] Step 1: ultrasonically clean a substrate coated with an anti-reflection film with an effective wavelength of 400 nm on one side using a 5% optical cleaning agent aqueous solution for 15 minutes, then clean the optical cleaning agent aqueous solution on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at 130° C. for drying;

[0059] Step 2, dissolving Sudan black in dimethylformamide at 0.5 wt % to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then placing the substrate on a test bench at 100° C. and heating it for 5 minutes to form an alignment layer;

[0060] Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation;

[0061] Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG1 84 at a mass ratio of 96:4 and dissolving them in a 15wt% toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern-programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating;

[0062] Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film;

[0063] Step 6: Using Sudan Black as a polarized light-absorbing dye, deposit it on the liquid crystal polymer film to form a polarized light-absorbing dye coating to obtain a microstructured polarizer.

[0064] Example 4

[0065] An embodiment of the present invention provides a method for preparing a microstructure polarizer, the method is used to prepare the above-mentioned microstructure polarizer based on the light-controlled orientation technology, and the method comprises the following steps:

[0066] Step 1: ultrasonically clean a substrate coated with an anti-reflection film with an effective wavelength of 400 nm on one side using a 5% optical cleaning agent aqueous solution for 15 minutes, then clean the optical cleaning agent aqueous solution on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at 130° C. for drying;

[0067] Step 2, dissolving a mixed solvent of AD1, Sudan III and Sudan black in dimethylformamide at 0.5 wt % to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then heating the substrate on a test bench at 100° C. for 5 min to form an alignment layer;

[0068] Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation;

[0069] Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 at a mass ratio of 96:4 and dissolving them in a 15wt% toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern-programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating;

[0070] Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film;

[0071] Step 6: Using a mixed solvent of AD1, sudan III and sudan black as a polarizing light absorbing dye, the mixed solvent is deposited on the liquid crystal polymer film to form a polarizing light absorbing dye coating to obtain a microstructure polarizer.

[0072] Example 5

[0073] A microstructured polarizer is prepared by the preparation method of a microstructured polarizer described in any one of embodiments 1 to 4.

[0074] Example 6

[0075] The microstructured polarizer prepared by the method of Example 1 is a composite material composed of a liquid crystal polymer as a "host" material and AD1 as a "guest" material. By utilizing the guest-host effect, the orientation of AD1 is related to the orientation of the liquid crystal polymer. The orientation layer is exposed to polarized light of a specific structured light beam to achieve a specific molecular axis long axis orientation of the liquid crystal molecules, thereby achieving a large-area orientation of AD1.

[0076] Practical applications require that the coatable polarizer has excellent polarization performance. The extinction ratio is an important parameter for characterizing linear polarizers. The extinction ratio is generally measured using a rotating analyzer, that is, the incident light from the light source passes through the depolarizer to be measured as a polarizer, then passes through a rotating analyzer, and is finally measured by a photodetector. When the transmission axis of the analyzer is aligned with the transmission axis of the depolarizer to be measured, the photodetector collects the maximum light power; when the transmission axis of the analyzer is orthogonal to the transmission axis of the depolarizer to be measured, the photodetector collects the minimum light power. The extinction ratio ER is the ratio of the maximum power to the minimum power.

[0077] pass Figure 3 It can be seen that when the direction of the AD1 molecules is parallel to the transmission axis of the analyzer, a large area of ​​uniform dark state is shown, and no blocky grainy rough film is formed. When the direction of the transmission axis of the rotating analyzer is perpendicular to the previous one, the dye molecules appear bright. The results show that the liquid crystal polymer after light curing under the new process of the present invention does not show obvious macroscopic disturbance of molecular orientation to the arrangement of AD1 molecules.

[0078] pass Figure 4 It can be seen that when building an extinction ratio test system in the present invention, the following requirements need to be paid attention to in sequence: the laser light source has a wavelength of 450nm; the LBTEK (APD 10-A) model achromatic quartz depolarizer is selected through the depolarizer, and the aperture is greater than 90% CA; the sample to be polarized is used as the polarizer; the polarizer is the thin film linear polarizer of LBTEK company, model: FLP25-VIS-M, extinction ratio>5000:1 (450nm-700nm); the photodetector: the PM100D digital optical power meter and the S120C model photodiode probe of Thorlabs company are selected, the optical power measurement wavelength range is 400-1000nm, and the energy range is 50nw-50mw.

[0079] Combination Figure 5 It can be seen that the extinction ratio of the AD1 polarizer is related to the thickness of the liquid crystal polymer film layer. By repeating steps 4 to 5 in Example 1, microstructured polarizers with different numbers of liquid crystal polymer film layers can be obtained. In the process of superimposing the number of liquid crystal polymer film layers, the extinction ratio of the AD1 polarizer increases with the increase in the number of liquid crystal polymer film layers. When the number of liquid crystal polymer film layers is 5, the thickness of the AD1 polarizer is 3.5μm and the extinction ratio is 336. The PE value calculated by the polarization efficiency expression of the polarizer is 99.7%, indicating that the polarizer can be used as a linear polarizer.

[0080] Example 7

[0081] The dye microarray polarizer sample with a sub-pixel size of 8μm×8μm was manufactured by laser direct writing technology, and the pattern of the polarizer collection device under the microscope was rotated for analysis. The molecular arrangement direction of the microarray in the four states of a superpixel unit was observed. When the incident polarization light was converted from 0 degrees to 90 degrees, the states corresponding to the mutually perpendicular micropolarization sub-pixels were interchanged. When the transmission axis of the polarizer was 0°, the maximum transmittance was displayed when the molecular arrangement direction of the azo dye was the same as the transmission axis of the polarizer; the minimum transmittance was displayed when the molecular arrangement direction of the azo dye was perpendicular to the transmission axis of the polarizer; when the angle between the two was 45° or 315°, the gray value of the unit was centered. When the polarizer was rotated 90°, the squares of maximum transmittance and minimum transmittance were interchanged, and the gray values ​​of 45° and 315° remained unchanged.

[0082] Combination Figure 6 It can be seen that the light source emits ultraviolet light through a polarization modulator to irradiate the photosensitive material located on the three-axis displacement stage. The response of the oriented material is controlled by changing the linear polarization angle of the exposure beam. Possible polarization control devices include half-wave plates or quarter-wave plates. It then passes through a spatial filter device and a collimating lens. Finally, the objective lens focuses the light beam on the substrate. The substrate on which the oriented material has been spin-coated can be placed on the displacement stage. The computer controls the moving direction of the displacement stage, and it can accurately align any position on the surface of the substrate, that is, the image to be projected is controlled by the computer. The laser direct writing system used in this example can achieve an exposure resolution of 1.5μm, the fast axis resolution accuracy of the liquid crystal molecules is + / -0.3°, the point-by-point orientation speed is 200HZ, the line-by-line orientation speed is 100mm / s, the ring-by-ring orientation is 240 turns / s, and the maximum orientation element diameter exceeds 12 inches.

[0083] Combination Figure 4 and Figure 7 It can be seen that in order to accurately measure the transmittance and extinction ratio to show the optical performance of the dye microarray device, a transmittance test device is used, the sample to be polarized is used as a polarizer, and the polarization device with a high extinction ratio is used as an analyzer. The analyzer is accurately rotated 360°, and the optical power data is recorded at intervals of 15°. It is calculated that the PE value of the unidirectional polarizer sample prepared by laser direct writing technology in this example at 450nm is 99.7%, and its extinction ratio is 336.

[0084] Example 8

[0085] Combination Fig. 9As shown in Figures a and b, based on the preparation steps of Example 1, the PDMS prepared by mixing the Sylgard 184 silicone elastomer with the curing agent at a ratio of 10:1 and then placing it in a vacuum for 30 minutes is spin-coated on the AD1 coating at a speed of 1000 r / min for 30 seconds. The PDMS silicone rubber is then cured at 120°C for 1 hour, and finally the sample is placed in deionized water for 3 minutes to obtain a flexible liquid crystal polymer film.

[0086] Combination Fig. 9 As shown in Figure c, the sample was subjected to a cyclic deformation test to determine the mechanical durability of the ultrathin flexible polarizer. At 21°C and 43% humidity, the bending radius was 1mm, and the flexible linear polarizer was bent continuously for 100 times, and the extinction ratio of the sample was measured at 450nm. When the number of folds increased to 300, the extinction ratio decreased slightly and then remained stable.

[0087] Combination Fig.10 It can be seen that the states of the microstructure polarizer prepared in Example 2 in the bright state and the dark state, as well as its extinction ratio in different wavelength bands.

[0088] Combination Fig.11 It can be seen that the states of the microstructure polarizer prepared in Example 3 in the bright state and the dark state, as well as its extinction ratio in different wavelength bands.

[0089] Combination Fig.12 It can be seen that the states of the microstructure polarizer prepared in Example 4 in the bright state and the dark state, as well as its extinction ratio in different bands.

[0090] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "examples", "specific examples", or "some examples" means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner.

[0091] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for preparing a microstructured polarizer, characterized in that: The preparation method comprises the following steps: Step 1: ultrasonically clean a substrate coated with an antireflection film on one side using an aqueous solution of an optical cleaning agent for a first preset time, then clean the aqueous solution of the optical cleaning agent on the substrate using acetone and alcohol, and place the cleaned substrate in an oven at a first preset temperature for drying; Step 2, dissolving the polarized light absorbing dye in dimethylformamide at a preset weight ratio to prepare an alignment solution, spin-coating the alignment solution on the cleaned substrate, and then placing the substrate on a test bench at a second preset temperature and heating it for a second preset time to form an alignment layer; Step 3, irradiating the alignment layer with linearly polarized ultraviolet light to obtain an alignment layer with a programmable structured polarized orientation; Step 4, mixing the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 and dissolving them in a toluene solution to prepare a liquid crystal polymer solution, and spin-coating the liquid crystal polymer on the pattern programmable structured polarization orientation orientation layer to obtain a liquid crystal polymer monomer coating; Step 5, using a photocuring process to process the liquid crystal polymer monomer coating to obtain a liquid crystal polymer film; Step 6: depositing a polarized light absorbing dye on the liquid crystal polymer film to form a polarized light absorbing dye coating to obtain a microstructured polarizer.

2. The method for preparing a microstructured polarizer according to claim 1, characterized in that: In the step 1, the effective wavelength band of the antireflection film is 400-700 nm, and the first preset time is 15-20 minutes.

3. The method for preparing a microstructured polarizer according to claim 2, characterized in that: In step 1, the first preset temperature is 50-200°C.

4. The method for preparing a microstructured polarizer according to claim 3, characterized in that: In the step 2, the weight ratio of the polarized light absorbing dye to dimethylformamide is 0.5 wt %.

5. The method for preparing a microstructured polarizer according to claim 4, characterized in that: In step 2, the second preset temperature is 50-200° C., and the second preset time is 1-60 min.

6. The method for preparing a microstructured polarizer according to claim 5, characterized in that: In step 4, the mixing mass ratio of the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 is 96:

4.

7. The method for preparing a microstructured polarizer according to claim 6, characterized in that: In step 4, the mass percentage of the mixture of the liquid crystal monomer RM57 and the ultraviolet light initiator IG184 and the toluene solvent is 15 wt %.

8. The method for preparing a microstructured polarizer according to claim 7, characterized in that: In step 6, the polarized light absorbing dye uses a mixed solvent of one or more of AD1, sudan III and sudan black.

9. A microstructured polarizer, characterized in that: The microstructured polarizer is prepared by the method for preparing a microstructured polarizer according to any one of claims 1 to 8.

10. An application of a microstructure polarizer, using the microstructure polarizer according to claim 9, characterized in that: The microstructure polarizer is used to capture polarization information of light.

Citation Information

Patent Citations

  • Composition for liquid crystal alignment layer, preparation method of liquid crystal alignment layer using the same, and optical film comprising the liquid crystal alignment layer

    CN101918513A

  • Display panel, manufacturing method of display panel and display device

    CN108388044A

  • Polarizer and manufacturing method thereof

    US20190072700A1

  • Optical film, elliptically polarizing plate, circularly polarizing plate, liquid crystal display element and method for manufacturing such optical film

    WO2006077723A1