Preparation method and application of graphite rod electrode
By extracting graphite negative electrode materials from waste lithium batteries, the problem of high energy consumption in lithium battery recycling and graphite rod production is solved, and high performance and low cost graphite rod electrode preparation is achieved, suitable for ore smelting and electricity Chemical applications.
Patent Information
- Application Number
- CN202410959397.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-19
AI Technical Summary
The existing lithium battery recycling methods have high energy consumption and high cost, and the high temperature energy consumption in graphite rod production leads to environmental pressure. The existing graphite rod electrode preparation process is complicated and energy is wasted.
Graphite rod electrodes are prepared by flotation, decomposition, drying, and calcination in waste lithium batteries. Combined with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and other materials, and obtained through extrusion molding and mechanical processing. Graphite rod electrode.
It reduces the energy consumption of graphite rod electrode production, alleviates the environmental pressure caused by the recycling of waste lithium batteries, improves the conductive performance of graphite rod electrodes, and has a simple preparation process and low cost.
Smart Images

Figure CN118983142A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of material recycling, and in particular to a preparation method of a graphite rod electrode and application thereof. Background Art
[0002] The recycling and treatment of lithium batteries has become a focus of attention today and in the future. At present, the methods used to recycle waste lithium batteries are divided into wet method, pyrolysis method and wet-pyrolysis method combined. However, the two methods have long recycling routes, high energy consumption and high cost, and the purity of the recovered products has certain limitations. For example, patent CN110724818B discloses a full wet recycling process for waste lithium batteries, including wet charged crushing, direct leaching of battery crushed materials, in-situ impurity removal of leachate, deep impurity removal and material re-preparation. The recycling method includes multiple steps, and the purity of the recovered materials is not enough and needs further processing during the reuse process.
[0003] Graphite rod electrodes are essential components for ore purification in electric arc furnaces. In the process of daily electric arc furnace smelting ore, an arc is generated between the end of the graphite rod electrode and the material in the furnace to convert electrical energy into thermal energy. Therefore, the high temperature generated is used as a heat source for smelting ore, melting the charge material for smelting. Typical examples are: yellow phosphorus, industrial silicon, abrasives, steel and other materials are smelted and purified using graphite electrodes in electric arc furnaces. However, in the existing graphite rod production, aggregates and binders are used for graphitization, which requires high temperature energy consumption, and the preparation process is complicated and wastes energy.
[0004] Therefore, how to use waste lithium batteries in electric arc furnace ore smelting to alleviate the environmental pressure caused by the accumulation of waste batteries and solve the problem that the existing graphite rod production has high energy consumption and is not conducive to environmental protection is a current key research topic. Summary of the invention
[0005] The main purpose of the present invention is to propose a preparation method of a graphite rod electrode and its application, aiming to provide a method for regenerating graphite negative electrode materials based on waste lithium batteries for making graphite rod electrodes, so as to reduce the high-temperature energy consumption required for graphitization of aggregates and binders in existing graphite rod production and the environmental pressure caused by the accumulation of waste batteries.
[0006] To achieve the above object, the present invention provides a method for preparing a graphite rod electrode, comprising the following steps:
[0007] S1. Using waste batteries as raw materials, dismantling them after discharging them, and separating the graphite negative electrode material from the copper foil in the dismantled waste batteries to obtain graphite negative electrode materials;
[0008] S2, immersing the graphite negative electrode material in an inorganic salt solution, performing flotation and impurity removal, and obtaining a graphite mixture;
[0009] S3, separating the graphite mixture into solid and liquid to obtain a solid graphite material, washing the graphite material, drying, and reducing to obtain graphite powder;
[0010] S4, mixing the graphite powder with ingredients, kneading to obtain slurry;
[0011] S5, extruding the slurry into a shape, drying it, and then calcining and graphitizing it to obtain a graphite rod;
[0012] S6. Mechanically process the graphite rod to obtain a graphite rod electrode.
[0013] Optionally, in step S2, the inorganic salt solution includes at least one of Na2CO3, NaHCO3, and NaOH; and / or,
[0014] The concentration of the inorganic salt solution is 20-100 g / L.
[0015] Optionally, in step S3, washing is performed using an ethanol solution; and / or,
[0016] The concentration of the ethanol solution is 40-70%.
[0017] Optionally, in step S3, the drying temperature is 60-120° C.; and / or,
[0018] The drying time is 8 to 24 hours.
[0019] Optionally, in step S3, the reducing agent includes at least one of glucose, chitosan and vitamin C; and / or,
[0020] The molar ratio of the graphite material to the reducing agent is 1:(1-3).
[0021] Optionally, in step S4, the ingredients are conductive carbon black, carbon nanotubes, polyvinylidene fluoride, coal tar pitch; and / or,
[0022] The mixing ratio of the graphite powder, conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch is 30:3:1:2:2.
[0023] Optionally, in step S4, the kneading method includes the following two steps:
[0024] S41, dry mixing, adding graphite powder, conductive carbon black, and carbon nanotubes into a container, stirring for 10 to 60 minutes to obtain a mixture;
[0025] S42, wet mixing, adding polyvinylidene fluoride solution and coal tar pitch into the mixture and wet mixing, wherein the wet mixing time is 30 to 90 minutes.
[0026] Optionally, in step S5, the extrusion molding pressure is 20-120 MPa; and / or,
[0027] The extrusion molding time is 60-300s; and / or,
[0028] The drying time is 8 to 24 hours; and / or,
[0029] The drying temperature is 80-150° C.; and / or,
[0030] The calcination temperature is 1700-1900° C.; and / or,
[0031] The calcination time is 25 to 35 minutes.
[0032] The present invention also provides a graphite rod electrode obtained by the preparation method of the graphite rod electrode as described above.
[0033] The present invention further proposes the application of the graphite rod electrode as described above in ore smelting and electrochemistry.
[0034] Compared with the prior art, the present invention has the following beneficial effects:
[0035] (1) Utilize the original components of graphite negative electrodes of waste lithium batteries to make graphite rod electrodes from graphite, conductive carbon black, carbon nanotubes, polyvinylidene fluoride, etc. This alleviates the environmental pressure brought by the recycling of waste batteries and saves the energy consumption of making graphite rod electrodes from asphalt and coal tar.
[0036] (2) The graphite rod electrode of the present invention has better conductivity than the graphite rod electrode made from the graphite negative electrode of waste lithium batteries.
[0037] (3) The process for making graphite rods of the present invention is simple, low in cost and has a good development prospect. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without paying creative work.
[0039] Figure 1 A schematic flow chart of an embodiment of a method for preparing a graphite rod electrode provided by the present invention;
[0040] Figure 2 It is a cyclic voltammetry curve of the graphite rod electrode in Example 1 of the present invention in 0.5 mol / L H2SO4.
[0041] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0042] To make the purpose, technical scheme and advantages of the embodiment of the present invention clearer, the technical scheme in the embodiment of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiment, it is carried out according to the normal conditions or the conditions recommended by the manufacturer. If the reagents or instruments used do not specify the manufacturer, they are all conventional products that can be purchased commercially. In addition, the meaning of "and / or" appearing in the full text includes three parallel schemes, taking "A and / or B" as an example, including scheme A, or scheme B, or schemes that A and B meet at the same time. In addition, the technical schemes between the various embodiments can be combined with each other, but must be based on the ability of ordinary technicians in the field to achieve. When the combination of technical solutions is contradictory or cannot be achieved, it should be considered that the combination of such technical solutions does not exist, and is not within the scope of protection required by the present invention. Based on the embodiments in the present invention, all other embodiments obtained by ordinary technicians in the field without making creative work belong to the scope of protection of the present invention.
[0043] In view of the environmental pressure caused by the accumulation of waste batteries and the high energy consumption of existing graphite rod production, which is not conducive to environmental protection, the present invention proposes a method for preparing graphite rod electrodes. Figure 1 , Figure 1 A schematic flow chart of an embodiment of a method for preparing a graphite rod electrode provided by the present invention comprises the following steps:
[0044] S1. Using waste batteries as raw materials, dismantling them after discharging them, and separating the graphite negative electrode material from the copper foil in the dismantled waste batteries to obtain graphite negative electrode materials;
[0045] S2, immersing the graphite negative electrode material in an inorganic salt solution, performing flotation and impurity removal, and obtaining a graphite mixture;
[0046] In this step, the inorganic salt solution includes at least one of Na2CO3, NaHCO3, and NaOH; the concentration of the inorganic salt solution is 20 to 100 g / L.
[0047] It should be noted that, for the purpose of achieving the present invention, the type of waste battery and the type of graphite are not limited, as long as they are graphite materials. In this embodiment, the waste battery used is a lithium iron phosphate battery with a specification of 3.2V and 280Ah, and the manufacturer is Yiyang Changtian New Energy Co., Ltd.
[0048] S3, separating the graphite mixture into solid and liquid to obtain a solid graphite material, washing the graphite material, drying, and reducing to obtain graphite powder;
[0049] In this step, the obtained graphite mixture is centrifuged at 8000-12000 r / min to separate impurities, and then a 0.1 μm pore size and an area of 0.65 m 2 , filter with a polytetrafluoroethylene filter membrane, and then use ethanol solution to wash the graphite material obtained after solid-liquid separation; the concentration of the ethanol solution is 40-70%, the concentration of the ethanol solution is preferably 55-70%, and more preferably 65%. Using ethanol within this concentration range for washing can fully remove impurities on the surface of the graphite material. The washed graphite material is dried at a temperature of 60-120°C; the drying time is 8-24h, and more preferably 10-12h at 75-90°C. The dried graphite material is then reduced, and the reducing agent includes at least one of glucose, chitosan, and vitamin C; the molar ratio of the graphite material to the reducing agent is 1:(1-3), and the molar ratio of the graphite material to the reducing agent is preferably 1:1.7.
[0050] S4, mixing the graphite powder with ingredients, kneading to obtain slurry;
[0051] In this step, the ingredients are conductive carbon black, carbon nanotubes, polyvinylidene fluoride, and coal tar pitch; the mixing ratio of the graphite powder, conductive carbon black, carbon nanotubes, polyvinylidene fluoride, and coal tar pitch is 30:3:1:2:2.
[0052] The kneading method comprises the following two steps:
[0053] S41, dry mixing, adding graphite powder, conductive carbon black, and carbon nanotubes into a container, stirring for 10 to 60 minutes, the dry mixing and stirring time is preferably 15 to 35 minutes, more preferably 20 to 25 minutes, to obtain a mixture;
[0054] S42, wet mixing, adding polyvinylidene fluoride solution and coal tar pitch into the mixture and wet mixing, the wet mixing time is 30 to 90 minutes, preferably 45 to 60 minutes.
[0055] S5, extruding the slurry into a shape, drying it, and then calcining and graphitizing it to obtain a graphite rod;
[0056] In this step, the slurry obtained after kneading is subjected to graphite rod extrusion molding, the pressure used for the extrusion molding is 20-120MPa; the extrusion molding time is 60-300s; after extrusion molding, it is dried, the drying time is 8-24h; the drying temperature is 80-150℃; after drying, it is roasted, the roasting temperature is 1700-1900℃; the roasting time is 25-35min. Preferably, the roasting procedure is to start from room temperature, increase the temperature to 1800℃ at 5℃ / min, and keep the temperature at 1800℃ for 30min, then start to cool at 5℃ / min, and cool to room temperature naturally after dropping to 400℃.
[0057] S6. Mechanically process the graphite rod to enhance the mechanical strength of the graphite rod to obtain a graphite rod electrode.
[0058] In this step, the mechanical processing includes graphite rod cutting, polishing and other processing to increase the electrical conductivity, heat transfer performance and mechanical properties of the graphite rod.
[0059] The present invention utilizes the original component materials of the graphite negative electrode of waste lithium batteries to make graphite rod electrodes from graphite, conductive carbon black, carbon nanotubes, polyvinylidene fluoride, etc., which alleviates the environmental pressure brought by the recycling of waste batteries and saves the energy consumption of making graphite rod electrodes from asphalt and coal tar. The present invention has a simple process for making graphite rod electrodes, low cost, and good development prospects.
[0060] The present invention also provides a graphite rod electrode obtained by the preparation method of the graphite rod electrode as described above. The graphite rod electrode provided by the present invention is made of the graphite negative electrode of waste lithium batteries, and its conductive performance is more superior in performance.
[0061] The present invention further proposes the application of graphite rod electrodes in ore smelting and electrochemistry. Graphite is a common negative electrode material for lithium batteries, accounting for 12-21% of the total content of the battery. By utilizing the characteristics of graphite materials that are easily separated from copper foil, the graphite negative electrode materials of waste batteries can be separately processed and recycled, which can reduce the recycling cost. In addition, recycling graphite materials from waste lithium batteries can effectively alleviate the environmental pressure and graphite mining pressure brought by waste lithium batteries. At present, most of the recycled graphite is used as raw materials for lithium batteries, which has high requirements for recycling technology and material purity. Therefore, it is necessary to start from other material perspectives and make graphite rod electrodes with recycled graphite for electric arc furnace ore purification.
[0062] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments and drawings. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0063] Example 1
[0064] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0065] (2) immersing the graphite negative electrode material in a solution of Na2CO3, NaHCO3, and NaOH for flotation and impurity removal to obtain a graphite mixture, wherein the molar ratio of Na2CO3, NaHCO3, and NaOH is 1:1:1, and the mass concentration of the mixed alkaline solution is 45 g / L;
[0066] (3) The graphite mixture was centrifuged at 8000 r / min to separate impurities, and then the graphite mixture was centrifuged at 8000 r / min to separate impurities. 2 , filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 70% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, glucose and vitamin C were selected as reducing agents to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the two reducing agents was 1:1:1;
[0067] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, i.e., graphite powder, conductive carbon black and carbon nanotubes are added and stirred. After dry mixing for 25 minutes, polyvinylidene fluoride solution is added and wet mixed for 50 minutes to obtain a slurry.
[0068] (5) extruding the slurry for 200 seconds at a pressure of 65 MPa, drying for 12 hours, and then calcining and graphitizing at a temperature of 80°C. The graphitization temperature is 1800°C for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800°C at 5°C / min, and maintaining the temperature at 1800°C for 30 minutes, and then starting to cool at 5°C / min, cooling to 400°C and then naturally cooling to room temperature;
[0069] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0070] Example 2
[0071] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0072] (2) immersing the graphite negative electrode material in a Na2CO3 and NaOH solution for flotation and impurity removal to obtain a graphite mixture, wherein the molar ratio of Na2CO3 and NaOH is 1:1, and the mass concentration of the mixed alkaline solution is 50 g / L;
[0073] (3) The graphite mixture was centrifuged at 10000 r / min to separate impurities, and then the graphite mixture was centrifuged at 10000 r / min to separate impurities. 2 , filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 65% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, glucose, chitosan, and vitamin C were selected as reducing agents to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the three reducing agents was 1:1:1:0.5;
[0074] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride, and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, that is, adding graphite powder, conductive carbon black, and carbon nanotubes and stirring. After dry mixing for 25 minutes, the polyvinylidene fluoride solution is added and wet mixed for 45 minutes to obtain a slurry.
[0075] (5) extruding the slurry for 100 seconds at a pressure of 55 MPa, then drying for 10 hours at a temperature of 100° C., and then calcining and graphitizing at a graphitization temperature of 1800° C. for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800° C. at 5° C. / min, and maintaining the temperature at 1800° C. for 30 minutes, and then starting to cool at 5° C. / min, cooling to 400° C. and then naturally cooling to room temperature;
[0076] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0077] Example 3
[0078] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0079] (2) immersing the graphite negative electrode material in a Na2CO3 and NaHCO3 solution, performing flotation and impurity removal, and obtaining a graphite mixture, wherein the molar ratio of the Na2CO3 and NaHCO3 is 1:2, and the mass concentration of the mixed alkaline solution is 50 g / L;
[0080] (3) The graphite mixture was centrifuged at 12000 r / min to separate impurities, and then the graphite mixture was centrifuged at 12000 r / min to separate impurities. 2, filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 65% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, vitamin C was selected as a reducing agent to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the vitamin C reducing agent was 1:3;
[0081] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, i.e., graphite powder, conductive carbon black and carbon nanotubes are added and stirred. After dry mixing for 25 minutes, polyvinylidene fluoride solution is added and wet mixed for 50 minutes to obtain a slurry.
[0082] (5) extruding the slurry for 300 seconds at a pressure of 50 MPa, then drying for 8 hours at a temperature of 120° C., and then calcining and graphitizing at a graphitization temperature of 1800° C. for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800° C. at 5° C. / min, and maintaining the temperature at 1800° C. for 30 minutes, and then starting to cool at 5° C. / min, cooling to 400° C. and then naturally cooling to room temperature;
[0083] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0084] Example 4
[0085] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0086] (2) immersing the graphite negative electrode material in a solution of Na2CO3, NaHCO3, and NaOH for flotation and impurity removal to obtain a graphite mixture, wherein the molar ratio of Na2CO3, NaHCO3, and NaOH is 1:1:1, and the mass concentration of the mixed alkaline solution is 45 g / L;
[0087] (3) The graphite mixture was centrifuged at 8000 r / min to separate impurities, and then the graphite mixture was centrifuged at 8000 r / min to separate impurities. 2 , filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 70% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, glucose and vitamin C were selected as reducing agents to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the two reducing agents was 1:1:1;
[0088] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, i.e., graphite powder, conductive carbon black and carbon nanotubes are added and stirred. After dry mixing for 25 minutes, polyvinylidene fluoride solution is added and wet mixed for 50 minutes to obtain a slurry.
[0089] (5) extruding the slurry for 200 seconds at a pressure of 65 MPa, drying for 12 hours, and then calcining and graphitizing at a temperature of 80°C. The graphitization temperature is 1800°C for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800°C at 5°C / min, and maintaining the temperature at 1800°C for 30 minutes, and then starting to cool at 5°C / min, cooling to 400°C and then naturally cooling to room temperature;
[0090] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0091] Example 5
[0092] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0093] (2) immersing the graphite negative electrode material in a solution of Na2CO3, NaHCO3, and NaOH for flotation and impurity removal to obtain a graphite mixture, wherein the molar ratio of Na2CO3, NaHCO3, and NaOH is 2:2:1, and the mass concentration of the mixed alkaline solution is 45 g / L;
[0094] (3) The graphite mixture was centrifuged at 8000 r / min to separate impurities, and then the graphite mixture was centrifuged at 8000 r / min to separate impurities. 2 , filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 50% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, chitosan was selected as a reducing agent to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the chitosan reducing agent was 1:3;
[0095] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, i.e., graphite powder, conductive carbon black and carbon nanotubes are added and stirred. After dry mixing for 25 minutes, polyvinylidene fluoride solution is added and wet mixed for 50 minutes to obtain a slurry.
[0096] (5) extruding the slurry for 200 seconds at a pressure of 80 MPa, drying for 24 hours, and then calcining and graphitizing at a temperature of 120° C. The graphitization temperature is 1800° C. for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800° C. at 5° C. / min, and maintaining the temperature at 1800° C. for 30 minutes, and then starting to cool at 5° C. / min, and cooling to 400° C. and then naturally cooling to room temperature;
[0097] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0098] Example 6
[0099] (1) using waste batteries as raw materials, discharging them after emptying them, and separating the graphite negative electrode material from the copper foil in the disassembled waste batteries to obtain the graphite negative electrode material;
[0100] (2) immersing the graphite negative electrode material in a Na2CO3 and NaOH solution for flotation and impurity removal to obtain a graphite mixture, wherein the molar ratio of Na2CO3 and NaOH is 1:1, and the mass concentration of the mixed alkaline solution is 70 g / L;
[0101] (3) The graphite mixture was centrifuged at 9000 r / min to separate impurities, and then the graphite mixture was centrifuged at 9000 r / min to separate impurities. 2 , filtered through a polytetrafluoroethylene filter membrane, and the obtained graphite powder was washed with a 70% ethanol solution to further remove impurities. Subsequently, it was dried at 80°C for 10 hours. Finally, glucose and vitamin C were selected as reducing agents to reduce the treated graphite material to obtain graphite powder, wherein the molar ratio of the graphite material to the two reducing agents was 1:2:1;
[0102] (4) mixing the graphite powder with conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch in a ratio of 30:3:1:2:2, and kneading. The kneading is divided into two steps. First, dry mixing is performed, i.e., graphite powder, conductive carbon black and carbon nanotubes are added and stirred. After dry mixing for 25 minutes, polyvinylidene fluoride solution is added and wet mixed for 50 minutes to obtain a slurry.
[0103] (5) extruding the slurry for 180 seconds at a pressure of 85 MPa, drying for 18 hours, and then calcining and graphitizing at a temperature of 100° C. The graphitization temperature is 1800° C. for 30 minutes to obtain a graphite rod, wherein the calcination process is carried out in a tubular furnace under argon gas protection, starting from room temperature, heating to 1800° C. at 5° C. / min, and maintaining the temperature at 1800° C. for 30 minutes, and then starting to cool at 5° C. / min, cooling to 400° C. and then naturally cooling to room temperature;
[0104] (6) Cutting and polishing the graphite rod to obtain a graphite rod electrode.
[0105] Comparative Example 1
[0106] The graphite rod electrode is prepared by graphitizing aggregate and binder.
[0107] Test methods and results
[0108] The graphite rod electrode prepared in Example 1 was placed in 0.5 mol / L H2SO4 and tested. The results are as follows: Figure 2 As shown, Figure 2 The cyclic voltammetry curves of the graphite rod electrode at different scan rates in 0.5 mol / L H2SO4 solution show that the cyclic voltammetry curves have a rectangular shape at different scan rates, indicating that the capacitance performance is ideal.
[0109] Industrial aluminum powder was placed in the graphite rod electrodes prepared in the above-mentioned Examples 1 to 6 and Comparative Example 1, and an aluminum melting test was carried out according to the metal melting standard. The maximum temperature was 720°C and the vacuum degree was 3.08×10~2Pa. During the aluminum melting process, the industrial aluminum powder melted into liquid aluminum and was coated on the center of the graphite rod electrode. After cooling and solidification, the graphite rod electrode was taken out to examine the demolding effect of the silicon block. The demolding effect was represented by the mass ratio of the remaining aluminum block bonded to the inside of the graphite rod electrode to the overall solidified aluminum. The results are shown in Table 1 below.
[0110] Table 1 Graphite rod electrode performance test table
[0111]
[0112] As can be seen from Table 1, the graphite rod electrodes in Examples 1 to 6 provided by the present invention have lower resistivity, greater flexural strength and elastic modulus, and are more conducive to electric furnace steelmaking or electrolytic purification.
[0113] In summary, the graphite rod electrode provided by the present invention uses waste batteries as raw materials, which alleviates the environmental pressure caused by the recycling of waste batteries, saves the energy consumption of making graphite rod electrodes from asphalt and coal tar, and has low resistivity, excellent heat transfer performance and high mechanical properties, and can be used in electric furnace steelmaking or electrolytic purification.
[0114] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing a graphite rod electrode, characterized in that: The following steps are involved: S1. Using waste batteries as raw materials, dismantling them after discharging them, and separating the graphite negative electrode material from the copper foil in the dismantled waste batteries to obtain graphite negative electrode materials; S2, immersing the graphite negative electrode material in an inorganic salt solution, performing flotation and impurity removal, and obtaining a graphite mixture; S3, separating the graphite mixture into solid and liquid to obtain a solid graphite material, washing the graphite material, drying, and reducing to obtain graphite powder; S4, mixing the graphite powder with ingredients, kneading to obtain slurry; S5, extruding the slurry into a shape, drying it, and then calcining and graphitizing it to obtain a graphite rod; S6. Mechanically process the graphite rod to obtain a graphite rod electrode.
2. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S2, the inorganic salt solution includes at least one of Na2CO3, NaHCO3, and NaOH; and / or, The concentration of the inorganic salt solution is 20-100 g / L.
3. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S3, washing with an ethanol solution; and / or, The concentration of the ethanol solution is 40-70%.
4. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S3, the drying temperature is 60-120° C.; and / or, The drying time is 8 to 24 hours.
5. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S3, the reducing agent includes at least one of glucose, chitosan and vitamin C; and / or, The molar ratio of the graphite material to the reducing agent is 1:(1-3).
6. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S4, the ingredients are conductive carbon black, carbon nanotubes, polyvinylidene fluoride, coal tar pitch; and / or, The mixing ratio of the graphite powder, conductive carbon black, carbon nanotubes, polyvinylidene fluoride and coal tar pitch is 30:3:1:2:
2.
7. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S4, the kneading method includes the following two steps: S41, dry mixing, adding graphite powder, conductive carbon black, and carbon nanotubes into a container, stirring for 10 to 60 minutes to obtain a mixture; S42, wet mixing, adding polyvinylidene fluoride solution and coal tar pitch into the mixture and wet mixing, wherein the wet mixing time is 30 to 90 minutes.
8. The method for preparing a graphite rod electrode according to claim 1, characterized in that: In step S5, the extrusion molding pressure is 20-120 MPa; and / or, The extrusion molding time is 60-300s; and / or, The drying time is 8 to 24 hours; and / or, The drying temperature is 80-150° C.; and / or, The calcination temperature is 1700-1900° C.; and / or, The calcination time is 25 to 35 minutes.
9. A graphite rod electrode obtained by the method for preparing a graphite rod electrode according to any one of claims 1 to 9.
10. Use of the graphite rod electrode as claimed in claim 9 in ore smelting and electrochemistry.