Power type precision alloy resistor and manufacturing method thereof
By employing a planar chip design and laser cutting and heat treatment of nickel-chromium alloy resistors, combined with silicone encapsulation and spot welding fixtures, the problems of large space occupation and poor heat dissipation of cylindrical resistors in precision instruments have been solved. This has resulted in high-precision, low-temperature drift, and pulse-resistant power resistors suitable for fields such as communications, computers, industrial control, and automobiles.
Patent Information
- Application Number
- CN202411122508.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-15
- Publication Date
- 2024-11-19
AI Technical Summary
Existing cylindrical power resistors occupy a large space in precision instruments, have poor heat dissipation, and low accuracy, which cannot meet the high precision and high stability requirements of lightweight and miniaturized equipment. Furthermore, they are prone to problems such as inductance generation and current unevenness under high power conditions.
The power precision alloy resistor adopts a planar chip design, uses a nickel-chromium alloy resistive element and high-temperature resistant 736 silicone encapsulation, and improves the density and anti-pulse capability of the resistive element through laser cutting and high-temperature heat treatment. Combined with spot welding fixtures, stable pin welding is achieved, and laser cutting compensation and grinding fine adjustment are used to control the resistance value accuracy.
It achieves high precision, low temperature drift, and non-inductive design, can operate stably under high power, has strong anti-pulse and anti-surge capabilities, improves the stability and heat dissipation of resistors, reduces the difficulty of operation and improves work efficiency.
Smart Images

Figure CN118983158A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of electronic components, and in particular to a power-type precision alloy resistor and a manufacturing method thereof. Background Art
[0002] With the widespread application of electronic equipment, including communications, computers, industrial control, automobiles, medical equipment, etc., the demand for resistors continues to increase. Especially in some precision instruments and equipment, power resistors have become indispensable key components because of their ability to withstand high power, high voltage and high current.
[0003] However, most of the power resistors on the market are cylindrical, and they use a large cylindrical design. When used in precision instruments and equipment, although they can achieve high power, their large size often determines that they occupy a large space. As equipment continues to become lighter and smaller, the market demand for high-precision, high-stability, and low-temperature drift high-power resistors is increasing. However, the high heat energy generated by small-sized resistors working at high power cannot be released, resulting in low stability, which can no longer meet market demand.
[0004] Therefore, there is an urgent need for a power-type precision resistor that not only meets the requirements of high precision, low temperature drift, and no inductance of precision resistors, but also has strong pulse and surge resistance and can operate stably under high power. Summary of the invention
[0005] The purpose of the present invention is to provide a power type precision alloy resistor, which solves the problem of low precision by laser cutting resistors, improves high temperature resistance by using high temperature resistant 736 type silicone packaging, uses nickel-chromium alloy for the resistor body, has high density and excellent line uniformity, can withstand the impact of large forward current, has strong anti-pulse ability and anti-surge ability, and has a low temperature drift characteristic by high temperature heat treatment at a set temperature during manufacturing; solves the problem of the influence of inductance on the resistor by chip design.
[0006] The purpose of the present invention can be achieved by the following technical solutions:
[0007] A power type precision alloy resistor, comprising two laminated ceramic substrates, a resistor body is encapsulated between the two ceramic substrates, the resistor body is encapsulated at one end of the ceramic substrate, both ends of the resistor body extend out of the end surfaces of the two ceramic substrates, and the extended resistor body part is symmetrically welded with pins;
[0008] The two ceramic substrates and the resistor body are packaged by bonding with silicon adhesive, and the resistor body is made of nickel-chromium alloy.
[0009] As a further solution of the present invention: the length of the resistor body is greater than the length of the ceramic substrate.
[0010] As a further solution of the present invention: the silicone adhesive is thermally conductive silicone.
[0011] As a further solution of the present invention: the nickel-chromium content ratio in the nickel-chromium alloy is 80:20.
[0012] As a further solution of the present invention: the nickel-chromium content ratio in the nickel-chromium alloy is 60:40.
[0013] As a further solution of the present invention: a method for manufacturing a power precision alloy resistor comprises the following steps:
[0014] Step 1: Laser cutting: Use a laser cutting machine to cut out the designed pattern and resistance value from the complete nickel-chromium alloy strip;
[0015] Step 2: High temperature heat treatment: subject the strip cut in step 1 to high temperature heat treatment at a temperature of 400°C to 620°C for 4 to 8 hours;
[0016] Step 3: Cutting: After the high temperature heat treatment is completed, the strip material after the high temperature heat treatment in step 2 is cut into individual resistors by a cutting device;
[0017] Step 4: Spot welding: Use a spot welding jig to lead out the electrodes at both ends of the resistor;
[0018] Step 5: Fine-tuning: Fine-tune the resistance value of the resistor by fine grinding and adjusting the resistance;
[0019] Step 6: Packaging: Print silicone adhesive on two ceramic substrates, place the resistor between the two ceramic substrates, and achieve fixed packaging of the resistor;
[0020] Step 7: Marking: inkjet and laser mark the ceramic substrate to obtain the finished resistor;
[0021] Step 8. Finished product inspection: Conduct precision test and appearance inspection on the finished resistors, and perform X-ray inspection on the products to ensure that there is no short circuit problem inside the products;
[0022] Step 9: Packaging: Pack qualified products.
[0023] As a further solution of the present invention: the spot welding fixture in step four includes a base plate, an electric guide rail assembly is arranged on one side of the top of the base plate, a mounting seat is installed on the electric slider of the electric guide rail assembly, a bearing base plate is installed on the top of the mounting seat, a processing groove is opened on one side of the bearing base plate, a welding base plate is installed on the top of the bearing base plate and above the processing groove, a welding cover plate is arranged on the top of the welding base plate, a support tube is arranged on the other side of the top of the base plate, the top of the support tube is connected to the bearing plate through a support rod, a cylinder is installed on the bearing plate, the telescopic rod of the cylinder passes through the bearing plate and is connected to a connecting rod, the bottom of the connecting rod is connected to a movable base, a fixed seat is symmetrically installed on the movable base and the base of the support tube, a connecting seat is connected to the fixed seat, and a spot welding head is installed on the connecting seat.
[0024] As a further solution of the present invention: a plurality of groups of placement grooves are arranged at equal intervals on the welding base plate for placing the resistor body and the pins.
[0025] As a further solution of the present invention: the specific welding process in step four is: place the cut single resistor body and pins into the placement groove, install the welding cover plate to position the resistor body and the pins on both sides, after positioning, move the welding base plate to the corresponding position through the electric guide rail assembly, start the cylinder to drive the spot welding head to move, and spot weld the resistor body and the pins on both sides.
[0026] Beneficial effects of the present invention:
[0027] 1. The present invention adopts a chip-type plane graphic design, and no circular current passes through, thus avoiding the generation of inductance value, realizing a non-inductive design of resistance value, and adopts a laser cutting compensation + grinding fine adjustment method, which can control the accuracy within ±0.05%. The cutting rough adjustment of resistance value is integrated through control compensation, which greatly reduces the work difficulty and improves work efficiency.
[0028] 2. The present invention uses high-temperature resistant 736-type silicone with high thermal conductivity to encapsulate the nickel-chromium alloy cut by laser inside two ceramic substrates. The nickel-chromium alloy resistor body is combined with the high thermal conductivity of the organic silicone and is completely in contact with the ceramic substrate, thereby achieving the resistor under high-power working conditions. Heat can be quickly evacuated through the ceramic substrate to maintain good stability.
[0029] 3. The present invention adopts spot welding jig for one-time forming, and can ensure that the contact area between the pin and the resistor body is fully welded, and the welding tension is ≥100N, which eliminates the risk of pin falling off and improves the stability of the product.
[0030] 4. The present invention can achieve a rated power of 3-10W based on the change of the outer dimensions. Laser cutting of alloy materials can ensure good line uniformity. The crystal structure inside the resistor body is dense, and there will be no inconsistent resistance line widths, which will cause overheating and melting at the intersection of the resistor body lines when the same current passes through. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] The present invention will be further described below in conjunction with the accompanying drawings.
[0032] Figure 1 It is a schematic diagram of the structure of the power precision alloy resistor of the present invention;
[0033] Figure 2 It is a schematic diagram of the side view structure of the power type precision alloy resistor of the present invention;
[0034] Figure 3 It is a schematic diagram of the top view of the spot welding fixture of the present invention;
[0035] Figure 4 It is a front view structural schematic diagram of the spot welding fixture of the present invention.
[0036] In the figure: 1. Ceramic substrate; 2. Resistor; 3. Pin; 4. Silicone adhesive; 100. Spot welding fixture; 10. Base plate; 11. Electric guide rail assembly; 12. Mounting seat; 13. Load-bearing base plate; 14. Processing groove; 15. Fixing seat; 16. Connecting seat; 17. Welding base plate; 18. Welding cover plate; 19. Placement groove; 20. Support tube; 21. Cylinder; 22. Connecting rod; 23. Moving base; 24. Spot welding head. DETAILED DESCRIPTION
[0037] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0038] The present invention Figure 1-Figure 4 As shown, a power type precision alloy resistor is designed, the resistor comprises two laminated ceramic substrates 1, and the ceramic substrate 1 is a rectangular sheet structure, a resistor body 2 is packaged between the two ceramic substrates 1, and the resistor body 2 is packaged at one end of the ceramic substrate 1, the length of the resistor body 2 is greater than the length of the ceramic substrate 1, and after packaging, the two ends of the resistor body 2 extend out of the end surfaces of the two ceramic substrates 1, and the extended part of the resistor body 2 is symmetrically welded with pins 3;
[0039] The two ceramic substrates 1 and the resistor 2 are packaged together using a silicone adhesive 4, and when the pins 3 are welded, a spot welding fixture 100 is used to lead out the electrodes at both ends.
[0040] Further, the silicone adhesive 4 is a thermally conductive silicone, including but not limited to high temperature resistant 736 type silicone. By using silicone with high thermal conductivity and good high and low temperature resistance, it is ensured that the resistor 2 can quickly release heat at high temperatures and can also operate stably at low temperatures.
[0041] Further the resistor body 2 is made of nickel-chromium alloy;
[0042] The nickel-chromium content ratio in the above nickel-chromium alloy is 80:20 or 60:40.
[0043] The internal resistor 2 of the present invention is made of alloy material, and has excellent compactness and line uniformity, can withstand instantaneous large current impact, and has strong pulse resistance and surge resistance.
[0044] The above-mentioned resistor manufacturing method further comprises the following steps:
[0045] Step 1, laser cutting: Use a laser cutting machine on the complete nickel-chromium alloy strip (where the nickel-chromium content ratio in the nickel-chromium alloy is 80:20 or 60:40), and adjust the cutting system of the laser cutting machine to compensate and cut out the designed graphics and resistance values (for example: the designed line width of the resistor 2 is 0.5mm, and the resistance value tested after cutting is 4.5Ω. According to calculation, the line width needs to be compensated by 0.070mm. The cutting compensation value can be directly modified on the laser machine without redrawing the drawing, which is more efficient). Finally, multiple resistors 2 with a resistance value 3%-10% lower than the target resistance are cut out;
[0046] Step 2, high temperature heat treatment: The resistor strip cut out in step 1 (a nickel-chromium alloy strip having a plurality of resistor bodies 2 with a resistance value 3%-10% lower than the target resistance) is subjected to high temperature heat treatment at a temperature of 400°C-620°C for 4-8 hours, and the temperature coefficient of the resistor body 2 is adjusted so that the TCR of the resistor body 2 is within ±20ppm in the range of (-55 to 125°C);
[0047] Step 3, cutting: After the high temperature heat treatment is completed, the resistor strip that has undergone the high temperature heat treatment in step 2 is cut into individual resistor bodies 2 by a cutting device;
[0048] Step 4, spot welding: Use the spot welding jig 100 to lead out the electrodes at both ends of the resistor 2; the existing electric welding technology requires two spot weldings for each pin 3, and there is a certain probability of the pin 3 being desoldered. The spot welding jig 100 of the present invention is formed by spot welding in one step, and can ensure that the contact area between the pin 3 and the resistor 2 is fully welded, and the welding tension is ≥100N, eliminating the risk of the pin 3 falling off, and improving the stability of the product;
[0049] Step 5: Fine adjustment: fine adjustment of the resistance value of resistor 2 is achieved through fine grinding and resistance adjustment;
[0050] Step 6: Packaging: Printing silicone adhesive 4 on two ceramic substrates 1, placing the resistor 2 between the two ceramic substrates 1, and implementing fixed packaging of the resistor 2; wherein the use of a planar package can ensure that the current of the resistor 2 has no loop circuit when the resistor 2 is working, thereby preventing the generation of inductance value;
[0051] Step 7: Marking: marking the ceramic substrate 1 by spraying code and laser marking to obtain a finished resistor;
[0052] Step 8. Finished product inspection: Conduct precision test and appearance inspection on the finished resistors, and perform X-ray inspection on the products to ensure that there is no short circuit problem inside the products;
[0053] Step 9: Packaging: Pack qualified products.
[0054] The manufacturing method of the present invention solves the problems of traditional power resistors that they occupy a large board area, have poor heat dissipation, low precision, and poor resistance-temperature characteristics. A laser-cut nickel-chromium alloy is encapsulated inside two ceramic substrates 1 of unlimited size (customized according to technical requirements) through a high-temperature resistant 736-type silicone with high thermal conductivity. The nickel-chromium alloy resistor body 2 is matched with the high thermal conductivity of the organic silicone and is completely in contact with the ceramic substrate 1, thereby achieving the goal that the resistor can quickly dissipate heat through the ceramic substrate 1 under high-power working conditions to maintain good stability.
[0055] Further Figure 3 and Figure 4 As shown, the spot welding fixture 100 in the above step 4 includes a base plate 10, an electric guide rail assembly 11 is arranged on one side of the top of the base plate 10, a mounting seat 12 is installed on the electric slider of the electric guide rail assembly 11, support blocks are symmetrically arranged on both sides of the top of the mounting seat 12, and a bearing base plate 13 is installed on the top of the two support blocks. A processing groove 14 is opened on one side of the bearing base plate 13, a welding base plate 17 is installed on the top of the bearing base plate 13 and above the processing groove 14, a welding cover plate 18 is arranged on the top of the welding base plate 17, and a plurality of groups of placement grooves 19 are arranged at equal intervals on the welding base plate 17 for The resistor body 2 and the pin 3 are placed, and a support cylinder 20 is arranged on the other side of the top of the bottom plate 10. The top of the support cylinder 20 is connected to a bearing plate through a support rod, and a cylinder 21 is installed on the bearing plate. The telescopic rod of the cylinder 21 penetrates the bearing plate and is connected to a connecting rod 22. The bottom of the connecting rod 22 is connected to a mobile base 23. The mobile base 23 and the base of the support cylinder 20 are symmetrically installed with a fixed seat 15, and the fixed seat 15 is connected to a connecting seat 16. A spot welding head 24 is installed on the connecting seat 16. The two spot welding heads 24 are arranged corresponding to the placement grooves 19 on the welding bottom plate 17, and are used to weld the pin 3 on the resistor body 2;
[0056] Further, the electric guide rail assembly 11 is a prior art, including an electric guide rail and an electric slider, to achieve horizontal movement of the welding base plate 17, which will not be described in detail here.
[0057] The specific welding process is:
[0058] Place the cut single resistor 2 and pin 3 into the placement groove 19, install the welding cover plate 18 to position the resistor 2 and the pins 3 on both sides, and after positioning, move the welding base plate 17 to the corresponding position (that is, the welding position of the resistor 2 and the pin 3 corresponds to the spot welding head 24) through the electric guide rail assembly 11, start the cylinder 21 to drive the spot welding head 24 to move, and spot weld the resistor 2 and the pins 3 on both sides. The spot welding is formed in one step to ensure that the contact area between the pin 3 and the resistor 2 is fully welded, and the welding tension is ≥100N, which eliminates the risk of the pin falling off and ensures the high stability and high temperature resistance of the resistor;
[0059] The products (resistor body 2 + pin 3) spot welded at different spot welding currents were subjected to tensile testing by conventional tensile testing method (gradually increasing tensile force applied until the weld joint breaks, thereby measuring the maximum tensile force that the weld joint can withstand before breaking, and the testing equipment is a tensile testing machine), and the welding tensile data are shown in Table 1 below.
[0060] Table 1:
[0061]
[0062]
[0063] It can be seen from the data in Table 1 that, using the spot welding method of the present invention, under the condition of a spot welding current of 1.9KA-2.1KA, the welding tension of the welded product is greater than 100N, and when the spot welding current is 2.0KA, the welding tension of the welded product is the best.
[0064] Furthermore, the accuracy of traditional cylindrical power resistors is relatively low, generally ≥0.5%, and due to the design of the annular resistor circuit, an inductance value will be generated when current passes through. This resistor has a small hindering effect on low-frequency alternating current, but a large hindering effect on high-frequency alternating current. As the stray inductance increases, the loss of resistance in the circuit will increase. Stray inductance may also cause oscillations, such as oscillations caused by sudden current changes, which may cause damage to the device due to electromagnetic interference or overvoltage limitations. It can be seen from the above-mentioned manufacturing method that the present invention adopts the method of laser cutting compensation + polishing fine adjustment, which can control the accuracy within ±0.05%, and adopts a chip-type planar graphic design, without a circular current passing through, avoiding the generation of inductance value, and achieving high-precision and non-inductive design of resistance value. And the integration of cutting and coarse adjustment of resistance value is realized by controlling compensation, which greatly reduces the difficulty of work and improves work efficiency.
[0065] Furthermore, the present invention performs a high temperature heat treatment of 400°C-620°C on the resistor body 2 (nickel-chromium alloy) (changing the crystal structure inside the alloy material at high temperature to release the stress of part of the crystal structure), and can achieve a good temperature coefficient of resistance (TCR) characteristic (-55-125°C) ≤±20ppm (while the temperature coefficient of the traditional power resistor is ≥50ppm). The specific test data are shown in Table 2 below:
[0066] Table 2
[0067]
[0068]
[0069] The heat treatment temperature in Table 2 above will be adaptively adjusted according to the product resistance and product material.
[0070] In summary, the present invention can provide a power-type precision alloy resistor which is high-precision, high-temperature resistant, has a low temperature coefficient (-55 to 125°C) ±20ppm, is non-inductive, has strong anti-pulse and anti-surge capabilities, and can operate stably under high power.
[0071] Compared with the screen-printed low-resistance resistors, the power is lower (0.1-1W). The rated power of the present invention can reach 3-10W according to the different external dimensions. The laser cutting alloy material can ensure good line uniformity. The crystal structure inside the resistor body is dense, and there will be no inconsistent resistance line width, which will cause overheating and melting in the narrow part of the resistor line when the same current passes through. The changes in materials and design make the present invention have strong pulse resistance and surge resistance.
[0072] In the description of the present invention, it should be understood that the terms "upper", "lower", "left", "right", etc. indicate directions or positional relationships based on the directions or positional relationships shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific direction, and a specific direction structure and operation, and therefore, cannot be understood as a limitation on the present invention. In addition, "first" and "second" are only for descriptive purposes, and cannot be understood as indicating or implying relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include one or more of the features. In the description of the present invention, unless otherwise specified, "multiple" means two or more.
[0073] In the description of the present invention, it should be noted that, unless otherwise clearly specified and limited, the terms "installed", "connected", "connected", etc. should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or an electrical connection; it can be a direct connection, or it can be an indirect connection through an intermediate medium, or it can be the internal communication of two components. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0074] The above is a detailed description of an embodiment of the present invention, but the content is only a preferred embodiment of the present invention and cannot be considered to limit the scope of implementation of the present invention. All equivalent changes and improvements made within the scope of the present invention should still fall within the scope of the patent coverage of the present invention.
Claims
1. A power type precision alloy resistor, characterized in that: The device comprises two laminated ceramic substrates (1), a resistor (2) being packaged between the two ceramic substrates (1), the resistor (2) being packaged at one end of the ceramic substrate (1), the two ends of the resistor (2) extending out of the end surfaces of the two ceramic substrates (1), and pins (3) being symmetrically welded to the extended portion of the resistor (2); The two ceramic substrates (1) and the resistor body (2) are packaged by bonding with each other using a silicon adhesive (4), and the resistor body (2) is made of a nickel-chromium alloy.
2. A power type precision alloy resistor according to claim 1, characterized in that: The length of the resistor (2) is greater than the length of the ceramic substrate (1).
3. A power type precision alloy resistor according to claim 1, characterized in that: The silicone adhesive (4) is heat-conducting silicone.
4. A power type precision alloy resistor according to claim 1, characterized in that: The nickel-chromium content ratio in nickel-chromium alloy is 80:
20.
5. The power type precision alloy resistor according to claim 1, characterized in that: The nickel-chromium content ratio in nickel-chromium alloy is 60:
40.
6. A method for manufacturing a power precision alloy resistor, characterized in that: The following steps are involved: Step 1: Laser cutting: Use a laser cutting machine to cut out the designed pattern and resistance value from the complete nickel-chromium alloy strip; Step 2: High temperature heat treatment: subject the strip cut in step 1 to high temperature heat treatment at a temperature of 400°C to 620°C for 4 to 8 hours; Step 3, cutting: After the high temperature heat treatment is completed, the strip material after the high temperature heat treatment in step 2 is cut into individual resistors (2) by a cutting device; Step 4: spot welding: using a spot welding jig (100) to lead out electrodes at both ends of the resistor (2); Step 5: Fine adjustment: fine adjustment of the resistance value of the resistor (2) is achieved by fine grinding and adjusting the resistance; Step 6: Packaging: Printing silicone adhesive (4) on two ceramic substrates (1), placing the resistor (2) between the two ceramic substrates (1), and achieving fixed packaging of the resistor (2); Step 7: Marking: marking the ceramic substrate (1) with inkjet printing or laser marking to obtain a finished resistor; Step 8. Finished product inspection: Conduct precision test and appearance inspection on the finished resistors, and perform X-ray inspection on the products to ensure that there is no short circuit problem inside the products; Step 9: Packaging: Pack qualified products.
7. The method for manufacturing a power precision alloy resistor according to claim 6, characterized in that: The spot welding jig (100) in step 4 comprises a base plate (10), an electric guide rail assembly (11) is arranged on one side of the top of the base plate (10), a mounting seat (12) is installed on the electric slider of the electric guide rail assembly (11), a bearing base plate (13) is installed on the top of the mounting seat (12), a processing groove (14) is opened on one side of the bearing base plate (13), a welding base plate (17) is installed on the top of the bearing base plate (13) and above the processing groove (14), and a welding cover plate (18) is arranged on the top of the welding base plate (17), A support tube (20) is arranged on the other side of the top of the bottom plate (10), the top of the support tube (20) is connected to a bearing plate via a support rod, a cylinder (21) is mounted on the bearing plate, a telescopic rod of the cylinder (21) penetrates the bearing plate and is connected to a connecting rod (22), a mobile base (23) is connected to the bottom of the connecting rod (22), a fixed seat (15) is symmetrically mounted on the mobile base (23) and the base of the support tube (20), a connecting seat (16) is connected to the fixed seat (15), and a spot welding head (24) is mounted on the connecting seat (16).
8. The method for manufacturing a power precision alloy resistor according to claim 7, characterized in that: A plurality of groups of placement grooves (19) are arranged at equal intervals on the welding bottom plate (17) for placing the resistor body (2) and the pins (3).
9. The method for manufacturing a power precision alloy resistor according to claim 8, characterized in that: The specific welding process in step 4 is as follows: the cut single resistor body (2) and pins (3) are placed in the placement groove (19), and the welding cover plate (18) is installed to position the resistor body (2) and the pins (3) on both sides. After positioning, the welding base plate (17) is moved to the corresponding position through the electric guide rail assembly (11), and the cylinder (21) is started to drive the spot welding head (24) to move, and the resistor body (2) and the pins (3) on both sides are spot welded.
Citation Information
Patent Citations
Foil-type precision resistor and manufacturing method thereof
CN103714926A
Sheet metal resistor and manufacturing method thereof
CN109841365A
Chip thin-film resistor network
CN112038026A
Intelligent segmentation spot welding device for alloy resistor
CN117711727A
Precision metal film resistor
CN204066915U