ThMn12 type magnet containing samarium element and preparation method thereof
By combining high-pressure die casting and coating, the problems of samarium volatilization and oxidation during the preparation of ThMn12 rare earth permanent magnets were solved, which improved the density and magnetic properties of the magnets and reduced the preparation cost.
Patent Information
- Application Number
- CN202411285060.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-13
- Publication Date
- 2024-11-19
AI Technical Summary
In the existing technology, the volatilization and oxidation of samarium in the preparation process of ThMn12 type rare earth permanent magnets have not been effectively solved, which affects the magnet performance and cost. In addition, traditional processes are difficult to maintain a low oxygen environment in high-temperature sintering furnaces.
By combining high pressure with coating, and through low-pressure pre-pressing, high-pressure die casting, and surface coating treatment, samarium volatilization is suppressed and oxidation is isolated, high-performance rare earth permanent magnets are prepared.
It significantly improves the density and magnetic properties of magnets, reduces porosity and defects, reduces samarium loss and oxidation, and optimizes the magnet manufacturing process.
Smart Images

Figure CN118983159A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of rare earth permanent magnet materials, and in particular to a rare earth permanent magnet material containing samarium element ThMn 12 Type magnet and preparation method thereof. Background Art
[0002] Permanent magnets are an essential component of modern industrial equipment and are widely used in many electrical / electronic devices such as computers, transportation and medical equipment. In the past few decades, with the emergence of rare earth (R) permanent magnets, the performance of permanent magnets has improved very rapidly. Now, common high-performance permanent magnets are almost all composed of rare earth permanent magnets. At the same time, given the global initiative to reduce carbon emissions, there is a surge in demand for cost-effective, high-performance and multifunctional magnets suitable for renewable energy systems. ThMn 12 Type based on SmFe 12-x M x Rare earth permanent magnets with ThMn components have become promising competitors due to their excellent magnetic properties, temperature stability, and reduced dependence on rare earth elements. However, as a samarium-based permanent magnet material, the volatility of samarium must be considered. Due to its low saturated vapor pressure, the loss of samarium during the magnet preparation process will inevitably destroy part of the magnet structure, reduce the performance of the magnet, and increase the cost of magnet preparation. Compared with other samarium-containing magnets such as samarium-iron-nitrogen and samarium-cobalt, ThMn 12 The metastable structure of ThMn exacerbates this volatility. Although sufficient attention has been paid to the research of samarium-containing magnets in the past, there is still no effective solution. In addition, most existing studies focus on ThMn 12 The fundamental aspects of structure and magnetic properties are only considered, while the related volatilization phenomena are neglected. This aspect has not received enough attention despite its important impact on the application of materials.
[0003] In addition, in the process of manufacturing samarium-containing magnets, in addition to the inevitable volatilization of samarium elements, the oxidation of the magnet itself is also a problem that must be taken seriously. In traditional processes, the solution to oxidation is generally to increase the oxygen content in the production environment as much as possible, including creating a vacuum and inert gas environment. However, it is still difficult to create an environment with a sufficiently low oxygen content in the industry, and this difficulty increases with the increase in production. Because ensuring the high airtightness of the high-temperature sintering furnace is not only costly, but also very difficult.
[0004] Therefore, the present invention proposes a method combining high pressure and coating to simultaneously solve the volatilization of the samarium element and the oxidation of the magnet, thereby effectively improving the magnetic properties of the magnet. Summary of the invention
[0005] In view of this, the present invention provides a samarium element ThMn 12The magnet and its preparation method can inhibit the volatilization of samarium and oxidation of the magnet during the preparation process, while optimizing the magnetic properties, and are of great research and application value.
[0006] The present invention is achieved by adopting the following technical solutions:
[0007] A samarium element ThMn 12 A method for preparing a type magnet comprises the following steps:
[0008] (1) Weigh samarium, iron, cobalt, and titanium metal elements in proportion and smelt them to obtain Sm(Fe 1-x Co x ) 11 Ti master alloy; among which Sm(Fe 1-x Co x ) 11 0≤x≤0.4 in Ti master alloy;
[0009] (2) Sm(Fe 0.8 Co 0.2 ) 11 Ti master alloy is subjected to belt spinning treatment to obtain Sm(Fe 1-x Co x ) 11 Ti amorphous crystal strips are ground for 1h to 2h and then passed through a 50-500 mesh sieve to obtain Sm(Fe 1-x Co x ) 11 Ti amorphous powder;
[0010] (3) Sm(Fe 1-x Co x ) 11 Ti amorphous powder is subjected to low-pressure pre-pressing die casting and high-pressure die casting to obtain a casting sheet;
[0011] (4) The cast sheet is coated with a coating, and the coated cast sheet is heat treated to obtain Sm(Fe 1-x Co x ) 11 Ti formed body;
[0012] (5) For Sm(Fe 0.8 Co 0.2 ) 11 The Ti formed body is quenched to obtain Sm(Fe 1-x Co x ) 11 Ti finished product, i.e. containing samarium element ThMn 12 Type magnet.
[0013] Preferably, the mass ratio of the samarium, iron, cobalt and titanium metal elements is 18.2-18.5: 44.6-75.6: 0-31.4: 5.8-5.9. The samarium element in the smelting material should be appropriately excessive by 10%-50% to cope with the inevitable large-scale volatilization of the samarium element during the high-temperature smelting process.
[0014] Furthermore, the smelting method is one of arc melting and induction melting.
[0015] Furthermore, the Sm(Fe 1-x Co x ) 11 Ti amorphous ribbons must eliminate the granular, linear, and plate-shaped parts that cannot be formed into a ribbon shape due to limitations of different equipment.
[0016] Further, the grinding is to grind Sm(Fe 1-x Co x ) 11 The Ti amorphous ribbon was ball milled in an oxygen-free environment.
[0017] Furthermore, step (2) is to use a belt spinning machine to perform belt spinning treatment in an inert gas atmosphere to prevent excessive oxidation. The main purpose of belt spinning is to obtain amorphous nanocrystalline ribbon sheets so as to obtain high-performance rare earth permanent magnet blocks later.
[0018] Preferably, the aperture of the quartz tube injection port of the belt spinning machine is 0.5mm-2mm, the relative injection pressure is 0.02MPa-0.08MPa, and the wheel speed is 40m / s-60m / s. It is necessary to ensure that the melt remains in a straight water column when flowing out of the injection port.
[0019] Preferably, the pressure of the low-pressure pre-casting in step (3) is 0.4 GPa to 1 GPa.
[0020] Preferably, the low-pressure pre-casting in step (3) can utilize a die-casting mold, and the die-casting mold can be made of hard steel, such as tungsten carbide, to ensure that it can repeatedly withstand a pressure of more than 1 GPa.
[0021] Preferably, the pressure of high pressure die casting in step (3) is 8 GPa to 15 GPa.
[0022] Preferably, in step (3), the high pressure die casting is to place the pre-pressed ingot into a restraining ring, and use a high pressure die casting device to perform high pressure treatment on the ingot and the restraining ring together. The high pressure die casting device and the restraining ring should maintain horizontal contact without forming a significant tilt angle, and the high pressure die casting device should fully consider whether it can withstand a pressure of more than 10GPa before die casting.
[0023] Furthermore, step (4) is to coat the cast sheet with a coating by evaporation or magnetron sputtering, wherein the inert metal includes Au, Ag, Pt, Mo, and Ta.
[0024] Preferably, the thickness of the coating is 5 nm to 20 nm.
[0025] Furthermore, the heat treatment is performed in an inert gas atmosphere or in a vacuum state at a temperature of 700 to 900°C.
[0026] Furthermore, the medium for the quenching treatment includes water, oil, and liquid nitrogen.
[0027] Another object of the present invention is to provide a high performance samarium-containing ThMn 12 Type magnet, comprising the above-mentioned samarium element ThMn 12 The preparation method of the type magnet is prepared, wherein the samarium element ThMn 12 The chemical formula of the magnet is as follows:
[0028] Sm(Fe 1-x Co x ) 11 Ti,
[0029] Among them, 0 <x≤0.4。
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention utilizes a combined method of low-pressure pretreatment and high-pressure treatment to significantly increase the content of samarium element ThMn 12 Type magnet Sm(Fe 1-x Co x ) 11 The density of Ti (0≤x≤0.4) is increased, which reduces the porosity, defects and oxygen inside it, thereby optimizing the magnetic properties.
[0032] 2. The present invention utilizes a surface coating method to form a samarium element ThMn 12 Type magnet Sm(Fe 1-x Co x ) 11 During the preparation process of Ti (0≤x≤0.4), the contact with external oxygen is isolated, thus avoiding oxidation of the magnet.
[0033] 3. The present invention uses a combination of high pressure and surface coating to convert the samarium element ThMn 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 Ti (0≤x≤0.4) is maintained in a high-density closed environment, which greatly reduces the magnetic performance and cost losses caused by the volatilization of samarium elements during the magnet preparation process. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] Figure 1 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 1-x Co x ) 11 Production flow chart of Ti (0≤x≤0.4);
[0035] Figure 2 Preparation of samarium-containing ThMn 12 Type magnet Sm(Fe 1-x Co x ) 11 Schematic diagram of the die casting mold and die casting method used in the Ti (0≤x≤0.4) process;
[0036] Figure 3 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 1-x Co x ) 11 Cross-sectional scanning electron microscope (SEM) image of Ti (0≤x≤0.4);
[0037] Figure 4 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 1-x Co x ) 11 Energy dispersive spectrum (EDS) analysis diagram of Ti (0≤x≤0.4);
[0038] Figure 5 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 1-x Co x ) 11 Detection diagram of mass change of Ti (0≤x≤0.4) during heat treatment;
[0039] Figure 6 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 1-x Co x ) 11 Magnetic properties data of Ti (0≤x≤0.4). DETAILED DESCRIPTION
[0040] The present invention will be further described below in conjunction with the embodiments.
[0041] Example 1
[0042] A samarium element ThMn 12 A method for preparing a type magnet comprises the following steps:
[0043] (1) Weigh 5.5 g Sm (excluding excess), 18.0 g Fe, 4.7 g Co, and 1.8 g Ti metal elements, mix them, and place them in an arc melting device for melting to obtain Sm (Fe 0.8 Co 0.2 ) 11 Ti master alloy;
[0044] (2) Sm(Fe 0.8 Co 0.2 ) 11 The Ti master alloy is placed in a belt spinning machine and spun in an inert gas atmosphere to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous ribbon, then Sm(Fe 0.8 Co 0.2 ) 11 The Ti amorphous ribbon was ball-milled in an oxygen-free environment for 1 h and sieved through a 500-mesh sieve to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous powder;
[0045] (3) First, Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous powder is placed in a die-casting mold for low-pressure pre-casting at a pressure of 1 GPa, then placed in a restraining ring and subjected to high-pressure die-casting at a pressure of 12.5 GPa using a high-pressure die-casting device, and then coated with Au (or Ag, Pt, Mo, Ta, etc.) elements by magnetron sputtering, and finally placed in a tube furnace and heated at 800°C in a vacuum environment for 15 minutes to obtain Sm (Fe 0.8 Co 0.2 ) 11 Ti formed body;
[0046] (4) Using water as quenching medium for Sm(Fe 0.8 Co 0.2 ) 11 The Ti formed body is quenched and finally Sm(Fe 0.8 Co 0.2 ) 11 Ti finished product, i.e. containing samarium element ThMn 12 Type magnet.
[0047] Comparative Example 1
[0048] A samarium element ThMn 12 A method for preparing a type magnet comprises the following steps:
[0049] (1) Weigh 5.5 g Sm (excluding excess), 18.0 g Fe, 4.7 g Co, and 1.8 g Ti metal elements, mix them, and place them in an arc melting device for melting to obtain Sm (Fe 0.8 Co 0.2 ) 11 Ti master alloy;
[0050] (2) Sm(Fe 0.8 Co 0.2 ) 11 The Ti master alloy is placed in a belt spinning machine and spun in an inert gas atmosphere to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous ribbon, then Sm(Fe 0.8 Co 0.2 ) 11 The Ti amorphous ribbon was ball-milled in an oxygen-free environment for 1 h and sieved through a 500-mesh sieve to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous powder;
[0051] (3) Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous powder was placed in a die casting mold for low-pressure pre-casting at a pressure of 1 GPa, and then placed in a tube furnace and heated at 800 ° C for 15 minutes in a vacuum environment to obtain Sm (Fe 0.8 Co 0.2 ) 11 Ti formed body;
[0052] (4) Using water as quenching medium for Sm(Fe 0.8 Co 0.2 ) 11 The Ti formed body is quenched and finally Sm(Fe 0.8 Co 0.2 ) 11 Ti finished product, i.e. containing samarium element ThMn 12 Type magnet.
[0053] Comparative Example 2
[0054] A samarium element ThMn 12 A method for preparing a type magnet comprises the following steps:
[0055] (1) Weigh 5.5 g Sm (excluding excess), 18.0 g Fe, 4.7 g Co, and 1.8 g Ti metal elements, mix them, and place them in an arc melting device for melting to obtain Sm (Fe 0.8 Co 0.2 ) 11 Ti master alloy;
[0056] (2) Sm(Fe 0.8 Co 0.2 ) 11 The Ti master alloy is placed in a belt spinning machine and spun in an inert gas atmosphere to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous ribbon, then Sm(Fe 0.8 Co 0.2 ) 11 The Ti amorphous ribbon was ball-milled in an oxygen-free environment for 1 h and sieved through a 500-mesh sieve to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti amorphous powder;
[0057] (3) First, Sm(Fe 0.8 Co 0.2 ) 11 The Ti amorphous powder was placed in a die casting mold for low-pressure pre-casting at a pressure of 1 GPa, then placed in a restraining ring and subjected to high-pressure die casting at a pressure of 12.5 GPa using a high-pressure die casting device, and then placed in a tubular furnace and heated at 800 °C in a vacuum environment for 15 minutes to obtain Sm(Fe 0.8 Co 0.2 ) 11 Ti formed body;
[0058] (4) Using water as quenching medium for Sm(Fe 0.8 Co 0.2 ) 11 The Ti formed body is quenched and finally Sm(Fe 0.8 Co 0.2 ) 11 Ti finished product, i.e. containing samarium element ThMn 12 Type magnet.
[0059] The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 of the present invention 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 The production process of Ti is as follows Figure 1 As shown, the present invention prepares the samarium element ThMn 12 Type magnet Sm(Fe 0.8 Co0.2 ) 11 Schematic diagram of the die casting mold and die casting method used in the Ti process Figure 2 shown.
[0060] like Figure 3 and 4 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 The cross-sectional scanning electron microscope (SEM) and energy spectrum (EDS) analysis diagram of Ti clearly show that the samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 Ti has obvious internal structure differences. 12 The internal pores of the magnet are significantly reduced compared with those of Comparative Example 1, and the fluctuation of the samarium element composition can be seen in the EDS analysis diagram. 12 There are almost no obvious internal defects and pores in the magnet, and there is almost no fluctuation in the samarium element composition. It is proved that the high pressure die casting + coating coating combined method of the present invention has a significant effect on inhibiting the volatilization of samarium elements in the magnet preparation process.
[0061] Figure 5 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 The mass change detection diagram of Ti during heat treatment. It can be seen from the figure that the samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 The difference between the two types of magnets is quite obvious. Among them, the mass increase is mainly due to oxidation, which means that the samarium element ThMn prepared in Comparative Example 1 12 There is a lot of oxidation in the magnet, while the samarium element ThMn prepared in Comparative Example 2 and Example 1 12 The oxidation in the magnet is greatly reduced, and the samarium element ThMn prepared in Example 1 12 The degree of oxidation in the magnet is reduced by more than 10 times compared with that in Comparative Example 1. Here, the specific degree of oxidation comparison is derived from the increase in the mass of the sample during the heating process. Figure 5The mass increase of Comparative Example 1 reached 17.8% and showed a rapid growth trend, while the mass increase of Example 1 was only 1.7%, and compared with Comparative Example 2, it also had a certain effect of reducing the mass increase. This means that the samarium element ThMn prepared in Example 1 12 Type magnets can greatly reduce the oxidation phenomenon of magnets during the manufacturing process.
[0062] Figure 6 The samarium-containing ThMn prepared in Comparative Example 1, Comparative Example 2 and Example 1 12 Type magnet Sm(Fe 0.8 Co 0.2 ) 11 Magnetic properties data of Ti. It can be seen that the overall magnetic properties of Example 1>Comparative Example 2>Comparative Example 1, that is, the samarium element ThMn prepared in Example 1 12 The magnetic properties of the magnets are significantly better than those of Comparative Examples 1 and 2, which proves that the preparation method of the present invention has a significant effect on optimizing the magnetic properties of magnets. This magnet optimization effect is achieved by suppressing the volatilization of samarium elements, the oxidation of samples, and optimizing the internal structure of samples during the magnet preparation process by combining high pressure die casting and coating coating in the present invention.
[0063] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A samarium element ThMn 12 A method for preparing a type magnet, characterized in that: The following steps are involved: (1) Weigh samarium, iron, cobalt, and titanium metal elements in proportion and smelt them to obtain Sm(Fe 1-x Co x ) 11 Ti master alloy; the Sm(Fe 1- x Co x ) 11 In Ti master alloy, 0≤x≤0.4; (2) The Sm(Fe 1-x Co x ) 11 Ti master alloy is subjected to belt spinning treatment to obtain Sm(Fe 1-x Co x ) 11 Ti amorphous crystal strips are ground for 1h to 2h and then passed through a 50-500 mesh sieve to obtain Sm(Fe 1-x Co x ) 11 Ti amorphous powder; (3) The Sm(Fe 1-x Co x ) 11 Ti amorphous powder is subjected to low-pressure pre-pressing die casting and high-pressure die casting to obtain a casting sheet; (4) coating the cast sheet with a coating, and heat treating the coated cast sheet to obtain Sm(Fe 1-x Co x ) 11 Ti formed body; (5) For the Sm(Fe 1-x Co x ) 11 The Ti formed body is quenched to obtain Sm(Fe 1-x Co x ) 11 Ti finished product, i.e. the samarium element ThMn 12 Type magnet.
2. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The mass ratio of the samarium, iron, cobalt and titanium metal elements is 18.2-18.5:44.6-75.6:0-31.4:5.8-5.
9.
3. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The smelting method is one of arc melting and induction melting.
4. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The grinding is to grind the Sm(Fe 0.8 Co 0.2 ) 11 The amorphous wafers were ball milled in an oxygen-free environment.
5. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: Step (2) is to use a belt spinning machine to 1-x Co x ) 11 The Ti master alloy is subjected to belt-spinning treatment in an inert gas atmosphere. The diameter of the quartz tube jet orifice of the belt-spinning machine is 0.5 mm to 2 mm, the jet relative pressure is 0.02 MPa to 0.08 MPa, and the wheel speed is 40 m / s to 60 m / s.
6. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The pressure of the low-pressure pre-casting in step (3) is 0.4 GPa to 1 GPa; the pressure of the high-pressure die-casting is 8 GPa to 15 GPa.
7. The samarium-containing element ThMn according to claim 1. 12 A method for preparing a type magnet, characterized in that: Step (4) is to coat the cast sheet with a coating by evaporation or magnetron sputtering, wherein the coating metal includes Au, Ag, Pt, Mo, Ta; and the thickness of the coating is 5nm to 20nm.
8. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The heat treatment in step (4) is to heat the cast sheet coated with the coating under inert gas or vacuum conditions, wherein the heating temperature is 700-900°C.
9. The samarium-containing element ThMn according to claim 1 12 A method for preparing a type magnet, characterized in that: The medium for the quenching treatment includes water, oil and liquid nitrogen.
10. A samarium element ThMn 12 Type magnet, characterized in that Prepared by any one of the methods of claims 1 to 9, the samarium element ThMn 12 The chemical formula of the magnet is as follows: Sm(Fe 1-x What x ) 11 You, Among them, 0 <x≤0.4。