Sintered permanent magnet and preparation method and application thereof

By forming a dual alloy process of M2Re phase and main alloy in NdFeB material, the problem of low solubility of Ti and Zr elements in NdFeB material is solved, the potential of the grain boundary phase and the corrosion resistance of the material are improved, and the reduction of the material is achieved. High corrosion resistance effect of magnetic properties.

CN118983160APending Publication Date: 2024-11-19YANTAI ZHENGHAI MAGNETIC MATERIAL CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411023874.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-29
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

When Ti and Zr elements are added to the existing NdFeB rare earth permanent magnet materials, the solubility is small and it is easy to generate additional precipitation phases with B, resulting in poor potential improvement effect of the grain boundary phase and it is difficult to improve the corrosion resistance of the material.

Method used

By forming a M2Re-rich phase in NdFeB material, M2 is Ti and/or Zr, uniformly distributed in the grain boundary phase, combining a dual alloy process of main alloy and auxiliary alloy, sintered permanent magnets are prepared to ensure that the content of M2 is above 1 wt%. , and through specific sintering and aging heat treatment processes, a uniformly distributed M2Re phase is formed.

Benefits of technology

The potential of the grain boundary phase is increased, the potential difference between the main phase and the grain boundary phase is reduced, and the corrosion resistance of the sintered permanent magnet is significantly improved, while maintaining magnetic properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983160A_ABST
    Figure CN118983160A_ABST
Patent Text Reader

Abstract

The invention discloses a sintered permanent magnet and a preparation method and application thereof, the sintered permanent magnet comprises a main phase and a grain boundary phase, the grain boundary phase comprises a Re-rich phase and an M2Re-rich phase, and M2 is Ti and / or Zr. According to the sintered permanent magnet, a special M2Re-rich grain boundary phase is formed in the secondary magnet through a double-alloy method, Ti and / or Zr elements are evenly distributed in the M2Re-rich phase, the potential of the grain boundary phase is improved, the potential difference between a main phase and the grain boundary phase is reduced, and the corrosion resistance of the sintered permanent magnet is improved while the magnetic performance is not reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of permanent magnets and preparation thereof, and in particular relates to a sintered permanent magnet and a preparation method and application thereof. Background Art

[0002] Neodymium iron boron (NdFeB) rare earth permanent magnet materials (or permanent magnets) are widely used in permanent magnet motors due to their high remanent magnetic density, high coercive force, high magnetic energy product and other characteristics. Due to the continuous improvement of market requirements for material quality and diversification of demand, improving the corrosion resistance of NdFeB rare earth permanent magnet materials and improving their surface protection technology have become the key to breaking through the engineering application of rare earth permanent magnet materials. In order to improve the corrosion resistance of NdFeB rare earth permanent magnet materials themselves, a small amount of highly corrosion-resistant metals are usually added to NdFeB rare earth permanent magnet materials during the smelting process for alloying, regulating the material composition and organization, thereby improving the corrosion resistance of the magnet itself.

[0003] The small amount of metal elements added will partially dissolve in the grain boundary phase, thereby increasing the potential of the grain boundary phase and reducing the potential between the grain boundary phase and Nd2Fe 14 However, the solubility of some metal elements, such as Ti and Zr, in the grain boundary phase is very small, and they are easy to form additional precipitation phases Ti-B phase and Zr-B phase with B element. Therefore, smelting and adding Ti and Zr elements cannot effectively improve the potential of the grain boundary phase, and it is difficult to achieve the maximum improvement effect on the corrosion resistance of NdFeB magnets. Summary of the invention

[0004] In order to improve the above technical problems, the present invention provides a sintered permanent magnet, which includes a main phase and a grain boundary phase; wherein the grain boundary phase includes a Re-rich phase and an M2Re-rich phase; wherein M2 is Ti and / or Zr; and Re is selected from one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb.

[0005] According to an embodiment of the present invention, the M2Re-rich phase contains M2, and M2 is uniformly distributed in the M2Re-rich phase, and the content of M2 in the M2Re-rich phase is not less than 1wt%. Preferably, the content of M2 in the M2Re-rich phase is 1-3wt%, for example, 1%, 1.5%, 2%, 2.5% or 3%.

[0006] According to an embodiment of the present invention, within any field of view (wherein, the arbitrary field of view refers to observing the sintered permanent magnet using EPMA or TEM), under a magnification of 2w to 20w times, a field of view in which at least 10 grain boundary phase grains can be observed, the area of ​​the Re-rich phase is S1, and the area of ​​the M2Re-rich phase is S2, satisfying: 20%≤S2 / (S1+S2)≤50%, preferably, 40%≤S2 / (S1+S2)≤47%.

[0007] According to an embodiment of the present invention, the composition of the sintered permanent magnet, calculated as 100% by mass, comprises:

[0008] R, 26 wt% to 35 wt%; R is a rare earth element, and R is selected from at least one of La, Ce, Pr, Nd, Pm, Sm, Eu, Gd, Tb, Dy, Ho, Er, Tm, Yb, Lu, Sc and Y;

[0009] B, 0.7wt%~1.1wt%;

[0010] Co, 0wt%~3.0wt%;

[0011] M, 0.05wt% to 4.0wt%; M is selected from at least one of Ga, Cu, Al, Zr and Ti;

[0012] The balance is iron and unavoidable impurities.

[0013] According to an embodiment of the present invention, the composition of the sintered permanent magnet, based on 100% by mass, includes R29wt% to 34wt%, for example, 29wt%, 30wt%, 31wt%, 32wt%, 33wt% or 34wt%.

[0014] According to an embodiment of the present invention, the composition of the sintered permanent magnet, based on 100% by mass, includes 0.8wt% to 1.0wt% of B, for example, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1.0wt%.

[0015] According to an embodiment of the present invention, the composition of the sintered permanent magnet, based on 100% by mass, includes Co, 0.1wt% to 1.0wt%; for example, 0.1wt%, 0.2wt%, 0.4wt%, 0.6wt%, 0.8wt%, 0.85wt%, 0.9wt%, 0.95wt% or 1.0wt%.

[0016] According to an embodiment of the present invention, the composition of the sintered permanent magnet, based on 100% by mass, includes M, 0.3wt% to 3.0wt%, for example, 0.3wt%, 0.4wt%, 0.5wt%, 1wt%, 2wt% or 3wt%.

[0017] According to an embodiment of the present invention, the main phase grains have an RTB type phase structure, for example, R2T 14 B-type crystal structure, wherein T is Fe. The present invention also provides a method for preparing a sintered permanent magnet, the method comprising:

[0018] The sintered permanent magnet is prepared by mixing and sintering a main alloy Re-Fe-MB without Ti and Zr and an auxiliary alloy Re-M1-M2;

[0019] Wherein, M is selected from one or more of Al, Ga, Cu, and Co;

[0020] M1 is selected from at least one of Al and Cu,

[0021] M2 is selected from at least one of Ti and Zr;

[0022] Re has the meaning as above.

[0023] According to an embodiment of the present invention, the main alloy Re-Fe-MB is Re a Fe 1-a-b-c M b B c , wherein: 28wt%≤a≤35wt%; 0wt%≤b≤5wt%; 0.8wt%≤c≤1.2wt%;

[0024] The auxiliary alloy Re-M1-M2 is Re d M1 e M2 f ,in:

[0025] 70wt%≤d≤85wt%;

[0026] 15wt%≤e+f≤30wt%;

[0027] 1wt%≤f≤10wt%.

[0028] Preferably, 29wt%≤a≤32wt%.

[0029] Preferably, 0.5 wt%≤b≤4 wt%.

[0030] Preferably, 0.9 wt%≤c≤1.1 wt%.

[0031] Preferably, 70 wt%≤d≤80 wt%.

[0032] Preferably, 18 wt % ≤ e + f ≤ 27 wt %.

[0033] Preferably, 5wt%≤f≤10wt%.

[0034] According to an embodiment of the present invention, the added mass of the auxiliary alloy Re-M1-M2 accounts for 1-5wt% of the total mass of the main alloy and the auxiliary alloy, for example, 1%, 2%, 3%, 4% or 5%.

[0035] Preferably, the mixing time of the main alloy Re-Fe-MB magnetic powder and the auxiliary alloy Re-M1-M2 magnetic powder is 1 to 5 hours.

[0036] According to an embodiment of the present invention, the method is: mixing the main alloy Re-Fe-MB magnetic powder and the auxiliary alloy Re-M1-M2 magnetic powder, pressing the obtained mixed magnetic powder into a shape, sintering, and performing aging heat treatment to obtain the sintered permanent magnet.

[0037] According to an embodiment of the present invention, the main alloy Re-Fe-MB magnetic powder is obtained by pulverizing the main alloy Re-Fe-MB quick-solidified flakes.

[0038] According to an embodiment of the present invention, the auxiliary alloy Re-M1-M2 magnetic powder is obtained by crushing the auxiliary alloy Re-M1-M2 quick-solidified flakes, and can also be obtained by mechanical alloying powder making, gas atomization powder making and other methods.

[0039] According to an embodiment of the present invention, the crushing step of the main alloy Re-Fe-MB quick-setting flakes specifically includes: the main alloy Re-Fe-MB quick-setting flakes are coarsely crushed by hydrogen explosion, stirred and mixed, and then crushed by ball milling and air flow milling, stirred and mixed to obtain magnetic powder. Exemplarily, the crushing step is as follows: take the main alloy Re-Fe-MB quick-setting flakes, firstly hydrogen explosion and coarse crushing, then stir the powder for 1-5h, mix, then ball mill for 1~5h, and then grind and crush by air flow mill to obtain the main alloy Re-Fe-MB magnetic powder of target particle size.

[0040] According to an embodiment of the present invention, the pulverizing step of the auxiliary alloy Re-M1-M2 quick-solidified flakes is the same as the pulverizing step of the main alloy Re-Fe-MB quick-solidified flakes.

[0041] According to an embodiment of the present invention, the raw materials for preparing the main alloy Re-Fe-MB quick-solidified sheet include:

[0042] Re, M, B and Fe;

[0043] Wherein, Re and M have the meanings as above;

[0044] The amount of each raw material added is based on Re a Fe 1-a-b-c M b B c Add in a stoichiometric ratio.

[0045] According to an embodiment of the present invention, the raw materials for preparing the auxiliary alloy Re-M1-M2 quick-solidified thin sheet include:

[0046] Re, M1 and M2,

[0047] Wherein, Re, M1 and M2 have the meanings as above;

[0048] The amount of each raw material added is based on Re d M1 e M2 f Add in a stoichiometric ratio.

[0049] According to an embodiment of the present invention, the quick-setting sheet is prepared by a method known in the art, for example, by a quick-setting belt-spinning technique. Exemplarily, the quick-setting sheet preparation method is as follows: the raw materials for the quick-setting sheet (including the raw materials for the quick-setting sheet of the main alloy Re-Fe-MB and the raw materials for the quick-setting sheet of the auxiliary alloy Re-M1-M2) are heated by electromagnetic induction in a vacuum or inert gas until they are melted (for example, the heating temperature is 1100-1500°C), kept warm for 10-60 minutes, and then poured onto the surface of a quenching roller, and then placed in a cooling barrel for further cooling to obtain a quick-setting sheet.

[0050] According to an embodiment of the present invention, the particle size of the mixed magnetic powder is 2-6 μm.

[0051] According to an embodiment of the present invention, the compression molding process is: fill the magnetic powder along the compression molding direction, and obtain the green body after magnetic field orientation molding. Preferably, the mixed magnetic powder is filled into the compression molding die.

[0052] Preferably, the magnetic field strength of the magnetic field is 2-5T, exemplified by 2T, 3T, 4T, 5T.

[0053] Preferably, the magnetic field orientation molding specifically comprises: performing orientation pressing in a magnetic field with a field strength of 2T, and then obtaining the green body after cold isostatic pressing.

[0054] According to an embodiment of the present invention, the sintering temperature is 1000-1050° C., and the sintering time is 2-6 hours.

[0055] According to an embodiment of the present invention, the process of aging heat treatment is: firstly, a first aging heat treatment is performed at 750-950° C. for 2-6 hours, and then a second aging heat treatment is performed at 450-650° C. for 2-6 hours.

[0056] According to the implementation scheme of the present invention, the specific process of sintering and aging heat treatment is: the obtained green body is heated to 1000-1050°C in a vacuum environment and kept warm for 2-6 hours for sintering, and after cooling, two stages of aging heat treatment are performed, the first stage is 750-950°C aging heat treatment for 2-6 hours, and the second stage is 450-650°C aging heat treatment for 2-6 hours to obtain the target product or target diffusion substrate.

[0057] According to an embodiment of the present invention, the method for preparing the sintered permanent magnet is specifically as follows:

[0058] (1) preparing a main alloy Re-Fe-MB quick-solidified sheet, and crushing the main alloy Re-Fe-MB quick-solidified sheet to obtain a main alloy Re-Fe-MB magnetic powder, and uniformly mixing the obtained main alloy Re-Fe-MB magnetic powder and auxiliary alloy Re-M1-M2 magnetic powder according to a certain proportion;

[0059] (2) Pressing: Filling the mixed magnetic powder of step (1) along the pressing direction, and obtaining a green body after magnetic field orientation molding;

[0060] (3) After the green body of step (2) is sintered and densified in a vacuum environment, an aging heat treatment is performed to obtain the sintered permanent magnet.

[0061] During the sintering process of the present invention, the auxiliary alloy Re-M1-M2 with a lower melting point melts first and fills the voids in the compact, which can reduce the sintering temperature. During the low-temperature (i.e., 1000-1050°C) sintering process, the diffusion of the B element is inhibited, and the segregation caused by the combination of the Ti element or Zr element in the auxiliary alloy and the B element in the main alloy is reduced. Therefore, after sintering, the auxiliary alloy Re-M1-M2 forms a Ti-rich and / or Zr-rich rare earth phase with uniform distribution of Ti and / or Zr, i.e., a M2Re-rich phase.

[0062] In the present invention, according to the binary phase diagram (see Figure 5 and Figure 6 ), since there is no intermediate phase between Re2 and M2, but there is an intermediate phase between Re2 and M1, the M1 element is introduced into the Re2-M2 alloy to form the Re2-M1-M2 alloy as an auxiliary alloy. For example, the Pr-Ti binary alloy is usually composed of α-Pr and α-Ti phases, and the distribution of Ti element is non-uniform at the microscopic level. By introducing Al into the Pr-Ti alloy, a Pr-Al-Ti ternary alloy can be formed. Since there is an intermediate phase between Pr-Al, Ti can replace part of the Al atoms in the Pr-Al solid solution zone to form a Pr-Al-Ti solid solution, so as to achieve uniform distribution of the Ti element in the auxiliary alloy, and finally form a Ti-rich Re phase (M2Re-rich phase).

[0063] The present invention also provides the use of the sintered permanent magnet, preferably used in a motor.

[0064] Beneficial effects of the present invention:

[0065] The sintered permanent magnet of the present invention forms a special M2Re-rich grain boundary phase (i.e., M2Re-rich phase) in the secondary magnet through a dual alloy method, wherein Ti and / or Zr elements are uniformly distributed in the M2Re-rich phase, thereby increasing the potential of the grain boundary phase and reducing the potential difference between the main phase and the grain boundary phase, thereby improving the corrosion resistance of the sintered permanent magnet without reducing the magnetic properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0066] Figure 1 This is the SEM image of Example 1.

[0067] Figure 2 This is the SEM image of Comparative Example 1.

[0068] Figure 3 This is the TEM image of Example 1.

[0069] Figure 4 This is the TEM image of Comparative Example 1.

[0070] Figure 5 It is the Pr-Ti binary phase diagram in the prior art.

[0071] Figure 6 It is the Pr-Al binary phase diagram in the prior art. DETAILED DESCRIPTION

[0072] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0073] Unless otherwise specified, the raw materials and reagents used in the following examples are commercially available or can be prepared by known methods.

[0074] Example 1

[0075] A method for preparing a sintered NdFeB magnet comprises the following steps:

[0076] (1) The raw materials are prepared according to the following proportions: Pr accounts for 6.2wt%, Nd accounts for 24.8wt%, Ga accounts for 0.2wt%, Al accounts for 0.05wt%, Cu accounts for 0.15wt%, Co accounts for 0.2wt%, B accounts for 0.94wt%, and the rest is Fe and impurities. The prepared materials are vacuum melted at 1420°C and kept warm for 15 minutes, then poured on the surface of a quenching roller, and then dropped into a water cooling barrel for cooling to obtain a main alloy flake;

[0077] (2) The raw materials are prepared according to the following proportions: Pr accounts for 70wt%, Al accounts for 20wt%, and Ti accounts for 10wt%. The prepared materials are vacuum melted at 1100°C and kept warm for 15 minutes, then poured on the surface of a quenching roller, and then dropped into a water cooling barrel for cooling to obtain PrCuTi auxiliary alloy flakes;

[0078] The composition ratio of the main alloy flakes and the auxiliary alloy flakes is shown in Table 1.

[0079] (3) Take the flakes from step (1) and (2), mix them according to the mass of the auxiliary alloy added being 2% of the total mass of the main alloy and the auxiliary alloy, and grind the mixed flakes by hydrogen explosion and ball milling, and then grind them by jet milling, with the target particle size being VMD = 3.3 μm.

[0080] (4) filling the magnetic powder of step (3) into a vacuum press mold, pressing and molding under a magnetic field strength of 2T, and obtaining a green body after cold isostatic pressing;

[0081] (5) The green body of step (4) is placed in a vacuum sintering furnace, heated to 1030°C and sintered for 4 hours. Then, the green body is subjected to a first aging treatment at 900°C for 4 hours and a second aging treatment at 550°C for 4 hours to obtain a Nd-Fe-B green body.

[0082] Magnetic properties test:

[0083] After the material skin is evenly removed, the Nd-Fe-B blank is processed into φ10*10 sample columns along the magnetizing direction for magnetic property testing.

[0084] Corrosion resistance test:

[0085] The Nd-Fe-B blank was processed into 10 φ10*10 sample columns along the magnetizing direction and subjected to 4 days of PCT test. The test conditions were 121°C, 100% RH, 2.0 Bar, PCT weight loss value = (mass after PCT - mass before PCT) / sample column surface area, and the average weight loss value of the 10 samples was taken.

[0086] Tissue Characterization:

[0087] Take samples of Nd-Fe-B blank to make EPMA or TEM samples, magnify them by 2w to 20w times, and there is at least one complete main phase or Re-rich phase in the observation field of view. Perform a surface scanning analysis of the element distribution including Ti and Zr elements on the observation field to observe whether Ti or Zr elements are precipitated in the main phase or Re-rich phase.

[0088] The test results are shown in Table 1.

[0089] Example 2

[0090] The preparation method of Example 2 is the same as that of Example 1, except that in step (2), the auxiliary alloy smelting ratio is 75wt% of Pr, 20wt% of Cu, and 5wt% of Zr.

[0091] Example 3

[0092] The preparation method of Example 2 is the same as that of Example 1, except that in step (3), the mass of the auxiliary alloy added is 5% of the total mass of the main alloy and the auxiliary alloy for mixing.

[0093] Comparative Example 1

[0094] Instead of using a dual alloy process with a main-auxiliary alloy ratio, all elements are directly added during smelting. In step (1), the raw materials are mixed according to the following ratio: Pr accounts for 7.5wt%, Nd accounts for 24.3wt%, Ga accounts for 0.2wt%, Al accounts for 0.45wt%, Cu accounts for 0.15wt%, Ti accounts for 0.2wt%, Co accounts for 0.2wt%, B accounts for 0.92wt%, and the rest is Fe and impurities. Through HD, air flow milling, pressing and sintering, a single alloy blank with the same composition as Example 1 is prepared.

[0095] Comparative Example 2

[0096] Instead of using a dual alloy process with a main-auxiliary alloy ratio, all elements are directly added during smelting. In step (1), the raw materials are mixed according to the following ratios: Pr accounts for 7.6wt%, Nd accounts for 24.3wt%, Ga accounts for 0.2wt%, Al accounts for 0.05wt%, Cu accounts for 0.55wt%, Zr accounts for 0.1wt%, Co accounts for 0.2wt%, B accounts for 0.92wt%, and the rest is Fe and impurities. A single alloy blank with the same composition as in Example 2 is prepared by HD, air flow milling, pressing and sintering.

[0097] Comparative Example 3

[0098] The preparation method of Comparative Example 1 is the same as that of Example 1, except that in step (3), the mass of the auxiliary alloy added is 0.5% of the total mass of the main alloy and the auxiliary alloy.

[0099] Comparative Example 4

[0100] The preparation method of Comparative Example 1 is the same as that of Example 1, except that in step (3), the mass of the auxiliary alloy added is 6% of the total mass of the main alloy and the auxiliary alloy.

[0101] Comparative Example 5

[0102] Comparative Example 5 is prepared in the same manner as Example 1, except that: in step (1), Pr accounts for 6.1wt%, Nd accounts for 24.8wt%, Ga accounts for 0.2wt%, Al accounts for 0.05wt%, Cu accounts for 0.15wt%, Co accounts for 0.2wt%, Ti accounts for 0.1wt%, B accounts for 0.94wt%, and the remainder is Fe and impurities; in step (2), Pr accounts for 75wt%, Al accounts for 20wt%, and Ti accounts for 5wt%.

[0103] The performance tests of the blank permanent magnets of Examples 2-3 and Comparative Examples 1-5 were the same as those of Example 1. The test results are shown in Table 1.

[0104] Table 1

[0105]

[0106] Figure 1 This is the SEM image of the product of Example 1. Figure 1 It can be seen that the product has Re-rich grain boundary phase and M2Re-rich grain boundary phase; Figure 1 Middle: Ti = 1.52wt% in M2Re-rich phase, Ti = 0.11wt% in Re-rich phase.

[0107] Figure 2 is the SEM image of Comparative Example 1, Figure 1 It can be seen that the product contains Re-rich grain boundary phase and M2 precipitation phase TiB2. Figure 2 In the M2 precipitated phase TiB2, Ti=61.28wt%, and in the Re-rich phase, Ti=0.36wt%.

[0108] Since Comparative Examples 1, 2 and 5 contain M2 precipitated phase, the S2 / (S1+S2) ratio cannot be directly calculated.

[0109] Figure 3 TEM image of Example 1. Figure 3 It can be seen that the M2Re-rich grain boundary phase and the Ti element are evenly distributed in the grain boundary phase.

[0110] Figure 4 TEM image of Comparative Example 1. Figure 4 It can be seen that the Re-rich grain boundary phase and the M2 precipitation phase, and the Ti element phase are non-uniformly distributed in the grain boundary phase, among which the red circle is the rod-like structured TiB2 phase (M2 precipitation phase).

[0111] From Table 1, we can see that:

[0112] From the comparison between Example 1 and Comparative Example 1, and between Example 2 and Comparative Example 2, it can be seen that when the blank composition is the same, when the dual alloy method is used, when Re-M1-M2 is added as auxiliary alloys to introduce Ti and Zr elements, the magnetic properties, Br and Hcj are increased compared to direct addition by smelting and single alloy blanks. Since the dual alloy method can allow less Re, Al, and Cu elements to enter the NdFeB main phase, and these elements will reduce the saturation magnetization intensity Ms of the main phase, thereby reducing Br, and the Al and Cu elements in the grain boundary phase can inhibit grain growth and increase Hcj. According to the corrosion resistance test, Example 1 has a lower average weight loss than Comparative Example 1, indicating that the dual alloy method improves the corrosion resistance of the product. Figure 3 From the distribution of Ti and Zr elements, it can be seen that the dual alloy method allows more Ti and Zr elements to be dissolved in the Re-rich phase, thereby reducing the precipitation of TiB2 and ZrB2 phases, thereby improving the corrosion resistance of the product.

[0113] From the comparison between Example 1 and Comparative Example 3, it can be seen that when the amount of auxiliary alloy added is less than 1%, theoretically, there should be a M2Re-rich phase in the magnet. However, perhaps because the addition ratio is too low, the M2Re-rich phase was not found in the actual detection, and the weight loss of the magnet was not significantly improved.

[0114] By comparing Example 1, Example 3 and Comparative Example 4, it can be seen that when the amount of auxiliary alloy added is increased, Br decreases and Hcj increases (Examples 1 and 3), but when the amount of auxiliary alloy added is greater than 5%, Hcj no longer increases significantly, and due to the high proportion of the magnet grain boundary phase, the weight loss of the magnet increases and the corrosion resistance deteriorates (Comparative Example 4).

[0115] By comparing Example 1 and Comparative Example 5, it can be seen that when the components in the magnet raw materials are equivalent, when the Ti element exists in the main alloy, segregation of the Ti element will appear in the grain boundary phase in the magnet, and the corrosion resistance will also be reduced (Comparative Example 5). When the Ti element is completely introduced by the auxiliary alloy, the main alloy does not contain Ti, and the Ti element is completely and evenly distributed in the M2Re-rich grain boundary phase (Example 1).

[0116] The above is an exemplary description of the embodiments of the present invention. However, the protection scope of the present invention is not limited to the above embodiments. Any modification, equivalent substitution, improvement, etc. made by those skilled in the art within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A sintered permanent magnet, It is characterized in that The sintered permanent magnet includes a main phase and a grain boundary phase; wherein the grain boundary phase includes a Re-rich phase and an M2Re-rich phase; wherein M2 is Ti and / or Zr; and Re is selected from one or more of Sm, La, Ce, Y, Nd, Pr, Ho, Gd, Dy, and Tb.

2. The sintered permanent magnet according to claim 1, It is characterized in that The M2Re-rich phase contains M2, and M2 is uniformly distributed in the M2Re-rich phase. The content of M2 in the M2Re-rich phase is not less than 1 wt%.

3. The sintered permanent magnet according to claim 1 or 2, It is characterized in that Within any field of view, wherein the arbitrary field of view refers to the field of view in which at least 10 grain boundary phase grains can be observed when observing the sintered permanent magnet using EPMA or TEM at a magnification of 2w to 20w times, the area of ​​the Re-rich phase is S1, and the area of ​​the M2Re-rich phase is S2, satisfying: 20%≤S2 / (S1+S2)≤50%.

4. The method for preparing a sintered permanent magnet according to any one of claims 1 to 3, It is characterized in that The method comprises: The sintered permanent magnet is prepared by mixing and sintering a main alloy Re-Fe-MB without Ti and Zr and an auxiliary alloy Re-M1-M2; Wherein, M is selected from one or more of Al, Ga, Cu, and Co; M1 is selected from at least one of Al and Cu, M2 is selected from at least one of Ti and Zr; Re has the meaning as defined in claim 1.

5. The method according to claim 4, It is characterized in that The main alloy Re-Fe-MB is Re a Fe 1-a-b-c M b B c , wherein: 28wt%≤a≤35wt%; 0wt%≤b≤5wt%; 0.8wt%≤c≤1.2wt%; The auxiliary alloy Re-M1-M2 is Re d M1 e M2 f ,in: 70wt%≤d≤85wt%; 15wt%≤e+f≤30wt%; 1wt%≤f≤10wt%.

6. The method according to claim 4, It is characterized in that The added mass of the auxiliary alloy Re-M1-M2 accounts for 1-5wt% of the total mass of the main alloy Re-Fe-MB and the auxiliary alloy Re-M1-M2; Preferably, the mixing time of the main alloy Re-Fe-MB magnetic powder and the auxiliary alloy Re-M1-M2 magnetic powder is 1 to 5 hours.

7. The method according to claim 4, It is characterized in that The method comprises: mixing main alloy Re-Fe-MB magnetic powder and auxiliary alloy Re-M1-M2 magnetic powder, pressing the obtained mixed magnetic powder into a shape, sintering, and performing aging heat treatment to obtain the sintered permanent magnet.

8. The method according to claim 7, It is characterized in that The particle size of the mixed magnetic powder is 2-6 μm; Preferably, the pressing process is as follows: filling magnetic powder along the pressing direction, and obtaining a green body after magnetic field orientation molding; Preferably, the magnetic field strength of the magnetic field is 2-5T.

9. The method according to claim 7, It is characterized in that The sintering temperature is 1000-1050°C and the sintering time is 2-6h; Preferably, the process of aging heat treatment is: firstly, a first aging heat treatment is performed at 750-950° C. for 2-6 hours, and then a second aging heat treatment is performed at 450-650° C. for 2-6 hours.