Preparation method and application of lithium supplement electrode of lithium battery
By preparing lithium battery supplementation electrodes, the problems of uneven lithium supplementation and safety hazards of lithium battery supplementation are solved, and lithium batteries with high Kulun efficiency and long cycle life are achieved, reducing costs and environmental impacts.
Patent Information
- Application Number
- CN202411076452.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-07
- Publication Date
- 2024-11-19
AI Technical Summary
The existing lithium battery supplementation method cannot evenly adsorb lithium supplementation agents, which poses safety hazards and small production productivity.
A lithium battery lithium supplement electrode preparation method is adopted to mix positive electrode active substances, lithium supplement agents, binders and conductive agents to form lithium supplement electrode slurry, and make a thin film through coating and roll pressing, avoiding lithium The direct use of powder reduces safety risks.
The high Coulombic efficiency and long cycle life of lithium batteries are achieved, reducing costs and environmental impacts, and avoiding the risk of spontaneous combustion of lithium powder.
Smart Images

Figure BDA0004982410030000051
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of new energy batteries, and in particular to a preparation method and application of a lithium battery lithium supplement electrode. Background Art
[0002] During the first charge of a lithium-ion battery, the organic electrolyte will be reduced and decomposed on the surface of the negative electrode such as graphite to form a solid electrolyte interface (SEI) film, which permanently consumes a large amount of lithium from the positive electrode, resulting in a low coulombic efficiency (ICE) of the first cycle, reducing the capacity and energy density of the lithium-ion battery. In order to solve this problem, it is necessary to replenish lithium in the lithium battery electrode, that is, to add lithium to the battery before the lithium-ion battery works to replenish lithium ions. The lithium source of the electrode material is supplemented by lithium replenishment to offset the irreversible lithium loss caused by the formation of the SEI film, so as to increase the total capacity and energy density of the battery.
[0003] The existing patent publication number CN114420915A proposes that before injecting the electrolyte, the lithium replenishing solution is injected into the lithium battery precursor to soak the pole piece to replenish the pole piece with lithium and then dry it. This method cannot evenly adsorb the lithium replenishing agent on the positive electrode or the negative electrode, thereby causing local lithium precipitation. Secondly, the lithium replenishing solvent is easy to cause thermal shrinkage of the diaphragm material during the drying process, thereby causing safety hazards; the existing patent publication number CN115911273A proposes that the negative electrode sheet of the negative electrode-free lithium battery replenishing lithium includes two parts: the negative electrode current collector and the lithium replenishing composite film, wherein the lithium replenishing composite film is composed of a first polymer, a second polymer, silicon dioxide particles and lithium powder. The lithium powder is extremely easy to spontaneously combust in the environment, which is extremely dangerous and has low mass production. Therefore, a preparation method and application of lithium battery lithium replenishing electrodes are needed to solve the above problems. Summary of the invention
[0004] The purpose of the present invention is to provide a preparation method and application of a lithium battery lithium supplement electrode to solve the problems existing in the prior art mentioned in the above background technology.
[0005] To achieve the above object, the present invention provides the following technical solutions:
[0006] A method for preparing a lithium battery lithium supplement electrode comprises the following steps:
[0007] S1: Weigh 90-99% of the total weight of the powder, the positive electrode active material, 1-5% of the lithium supplement, 1-5% of the binder A, 1-5% of the binder B and 1-5% of the conductive agent, stir and mix for 0.5-1h, the speed is 500-1000r / min, the stirring temperature is 10-60℃, and mix evenly;
[0008] S2: Add 44% of the total weight of the cathode solvent, 0.1-1% of the dispersant, and 0.5-2% of the conductive agent to the material obtained in S1, and stir and mix for 0.5-2h at a speed of 500-2000r / min and a stirring temperature of 10-60°C;
[0009] S3: adding 6% of the total weight of the powder into the material obtained in S2, stirring and mixing for 0.5-5h, with a rotation speed of 1000-3000r / min and a stirring temperature of 10-60°C, to obtain a lithium supplement electrode slurry;
[0010] S4: The slurry obtained in S3 is uniformly coated on the current collector at 10-120° C. by a coating machine to obtain an active material sheet with a thickness of 100-300 μm;
[0011] S5: rolling the thin sheet obtained in S4 at 50-130° C. into an active material film of 40-150 μm to obtain a lithium battery lithium supplement electrode.
[0012] Preferably, the lithium supplement in S1 includes passivated lithium powder particles and a coating layer coated on the surface of the passivated lithium powder particles, the passivated lithium powder particles include one or more of lithium iron oxide, lithium nickel oxide, and lithium oxide, and the coating layer includes one or more of lithium carbonate, lithium phosphate, and lithium fluoride.
[0013] Preferably, the positive electrode active material in S1 includes one or more of lithium iron phosphate, lithium cobalt oxide, and lithium manganese iron phosphate.
[0014] Preferably, the binder A and the binder B in S1 are selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, acrylic resin, and styrene-butadiene rubber.
[0015] Preferably, the conductive agents in S1 and S2 are one or more of carbon nanotubes, graphene, carbon black, and acetylene black.
[0016] Preferably, the dispersant in S2 includes one or both of polyvinyl pyrrolidone and hexadecyltrimethylammonium bromide.
[0017] The invention discloses an application of a lithium replenishing electrode prepared by a method for preparing a lithium replenishing electrode for a lithium battery, wherein the lithium replenishing electrode is applied to a lithium battery.
[0018] Compared with the prior art, the present invention has the following beneficial effects:
[0019] The lithium replenishing coating of the present invention is prepared by adding a lithium replenishing agent when preparing the positive electrode slurry, and then releasing the lithium source through a high voltage during the subsequent formation, thereby avoiding the safety risks and equipment costs caused by lithium replenishment with lithium powder. The lithium replenishing electrode has the characteristics of low cost, environmental protection, and good conductivity, and replenishes the lithium consumed in the cycle process for the negative electrode active material, thereby achieving high coulomb efficiency and long cycle life of the battery. DETAILED DESCRIPTION
[0020] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.
[0021] The present invention provides the following technical solutions:
[0022] Example 1
[0023] A method for preparing a lithium battery lithium supplement electrode comprises the following steps:
[0024] S1: Weigh 95wt% lithium iron phosphate, 0wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 1wt% carbon black conductive agent, and 1wt% dispersant, stir and mix for 0.75h at a speed of 800r / min and a stirring temperature of 25°C until the mixture is evenly mixed;
[0025] S2: Add 44% of the total weight of the cathode solvent (total solid content 75%) and 1% of the carbon nanotube conductive agent to the material obtained in S1, and stir and mix for 1.5 hours at a speed of 1000 r / min and a stirring temperature of 25°C;
[0026] S3: Add 6% of the total weight of the cathode solvent (overall solid content 64%) to the material obtained in S2, stir and mix for 3 hours at a speed of 2000 r / min and a stirring temperature of 25° C. to obtain a lithium supplement electrode slurry;
[0027] S4: The slurry obtained in S3 is uniformly coated on the current collector at 105° C. by a coater to obtain an active material sheet with a thickness of 220 μm;
[0028] S5: The thin sheet obtained in S4 is rolled at 65° C. to form an active material film of 150 μm to obtain a lithium battery lithium supplement electrode.
[0029] In the present invention, it is necessary to add the solvent step by step. The step-by-step addition of the solvent allows the binder to be fully kneaded with the dry powder to form a better dispersion. Steps S1, S2 and S3 cannot be replaced arbitrarily. The passivated lithium powder is added first because the passivated lithium powder is easier to agglomerate than the conductive agent. The dispersant is added first to allow the positive electrode active material to fully contact with the binder and the passivated lithium powder. The dispersant added then mainly plays a role of lubrication and dispersion. The solvent added further promotes the dispersion of each active substance.
[0030] Compared with the introduction of pure lithium powder, lithium carbonate / lithium phosphate coated passivated lithium powder is easier to store and has lower environmental requirements. At the same time, in the early stage of the cycle, pure lithium powder releases lithium ions quickly, which can easily lead to excessive enrichment of lithium ions, causing irreversible lithium precipitation, thereby worsening the cycle. The lithium carbonate and lithium phosphate coating layers make the release of lithium ions continuous and slow, and are not easy to cause lithium precipitation. To avoid lithium precipitation, the ratio of passivation lithium powder added to the total weight of the powder should be less than the positive electrode active material * the ratio of the positive electrode active material to the total weight of the powder * (1-the first coulombic efficiency of the full battery without lithium supplementation) / passivation lithium powder gram capacity * 1.15.
[0031] Example 2
[0032] The only difference from Example 1 is the addition ratio of each raw material, 94wt% lithium iron phosphate, 1wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 1wt% carbon black conductive agent, 1wt% dispersant, and 1wt% carbon nanotube conductive agent.
[0033] Example 3
[0034] The only difference from Example 1 is the addition ratio of each raw material, 93wt% lithium iron phosphate, 2wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 1wt% carbon black conductive agent, 1wt% dispersant, and 1wt% carbon nanotube conductive agent.
[0035] Example 4
[0036] The only difference from Example 1 is the addition ratio of each raw material, 92wt% lithium iron phosphate, 3wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 1wt% carbon black conductive agent, 1wt% dispersant, and 1wt% carbon nanotube conductive agent.
[0037] Example 5
[0038] The only difference from Example 1 is the addition ratio of each raw material, 91wt% lithium iron phosphate, 4wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 1wt% carbon black conductive agent, 1wt% dispersant, and 1wt% carbon nanotube conductive agent.
[0039] Example 6
[0040] The only difference from Example 1 is the addition ratio of each raw material, 92wt% lithium iron phosphate, 3wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 0.5wt% carbon black conductive agent, 1wt% dispersant, and 1.5wt% carbon nanotube conductive agent.
[0041] Example 7
[0042] The only difference from Example 1 is the addition ratio of each raw material, 92wt% lithium iron phosphate, 3wt% lithium carbonate-coated passivated lithium powder, 1wt% binder A, 1wt% binder B, 0wt% carbon black conductive agent, 1wt% dispersant, and 2wt% carbon nanotube conductive agent.
[0043] The positive electrode sheets of Examples 1-7 were respectively assembled into batteries with the same negative electrode sheets, separators, and electrolytes.
[0044] Table 1 shows the first coulombic efficiency of the battery prepared with the positive electrode material, the gram capacity of the positive electrode material and the capacity retention rate after 1500 cycles:
[0045] Table 1
[0046]
[0047] As can be seen from Table 1, Example 4 prepared in Examples 1-5 of the present invention shows higher first coulombic efficiency, gram capacity utilization and better cycle performance; Compared with Example 4, Example 6 optimizes the conductive agent formula to improve the cycle capacity retention rate; Therefore, the method adopted by the present invention can prepare a lithium battery with higher first coulombic efficiency, gram capacity utilization and better cycle performance.
[0048] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a lithium battery lithium supplement electrode, It is characterized in that The steps include: S1: Weigh 90-99% of the total weight of the powder, the positive electrode active material, 1-5% of the lithium supplement, 1-5% of the binder A, 1-5% of the binder B and 1-5% of the conductive agent, stir and mix for 0.5-1h, the speed is 500-1000r / min, the stirring temperature is 10-60℃, and mix evenly; S2: Add 44% of the total weight of the cathode solvent, 0.1-1% of the dispersant, and 0.5-2% of the conductive agent to the material obtained in S1, and stir and mix for 0.5-2h at a speed of 500-2000r / min and a stirring temperature of 10-60°C; S3: adding 6% of the total weight of the powder into the material obtained in S2, stirring and mixing for 0.5-5h, with a rotation speed of 1000-3000r / min and a stirring temperature of 10-60°C, to obtain a lithium supplement electrode slurry; S4: The slurry obtained in S3 is uniformly coated on the current collector at 10-120° C. by a coating machine to obtain an active material sheet with a thickness of 100-300 μm; S5: rolling the thin sheet obtained in S4 at 50-130° C. into an active material film of 40-150 μm to obtain a lithium battery lithium supplement electrode.
2. A method for preparing a lithium battery lithium supplement electrode according to claim 1, Features: The lithium supplement in S1 includes passivated lithium powder particles and a coating layer coated on the surface of the passivated lithium powder particles, the passivated lithium powder particles include one or more of lithium iron oxide, lithium nickel oxide, and lithium oxide, and the coating layer includes one or more of lithium carbonate, lithium phosphate, and lithium fluoride.
3. The method for preparing a lithium battery lithium supplement electrode according to claim 1, Features: The positive electrode active material in S1 includes one or more of lithium iron phosphate, lithium cobalt oxide, and lithium manganese iron phosphate.
4. The method for preparing a lithium battery lithium supplement electrode according to claim 1, Features: In the S1, the binder A and the binder B are selected from one or more of polyvinylidene fluoride, polytetrafluoroethylene, acrylic resin, and styrene-butadiene rubber.
5. The method for preparing a lithium battery lithium supplement electrode according to claim 2, Features: The conductive agents in S1 and S2 are one or more of carbon nanotubes, graphene, carbon black, and acetylene black.
6. The method for preparing a lithium battery lithium supplement electrode according to claim 2, It is characterized in that The dispersant in S2 includes one or both of polyvinyl pyrrolidone and hexadecyltrimethylammonium bromide.
7. An application of a lithium-supplementing electrode prepared by the method for preparing a lithium-supplementing electrode for a lithium battery according to any one of claims 1 to 6, It is characterized in that The lithium supplement electrode is applied to a lithium battery.