Pre-lithium composite diaphragm, lithium ion battery and preparation method

By filling the voids in the separator matrix with polymer material in a pre-lithiated composite separator, the problem of lithium consumption during lithium-ion battery assembly is solved, improving lithium replenishment efficiency and cell performance, while reducing production costs.

CN118983619AActive Publication Date: 2024-11-19ADVANCED MATERIALS TECH (BEIJING) CO LTD

Patent Information

Application Number
CN202411189389.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-11-19
Estimated Expiration
2044-08-28

AI Technical Summary

Technical Problem

In existing lithium-ion battery lithium replenishment separators, lithium is easily consumed by reacting with air during assembly, affecting lithium replenishment efficiency. Furthermore, the existing protective layer reduces the separator porosity and increases its thickness, affecting cell performance and cost.

Method used

Polymer material is filled into the voids of the membrane matrix to form a pre-lithiation composite membrane. The polymer dissolves and swells in the electrolyte to protect the pre-lithiation layer and is produced continuously in an open environment.

Benefits of technology

It effectively protects the pre-lithiation layer, reduces lithium consumption, maintains or improves ionic conductivity and volumetric energy density, reduces production costs, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118983619A_ABST
    Figure CN118983619A_ABST
Patent Text Reader

Abstract

The invention provides a pre-lithium composite diaphragm, a lithium ion battery and a preparation method, and belongs to the field of batteries. The pre-lithium composite diaphragm comprises a diaphragm substrate, a filling material, a pre-lithium layer and a protective layer, gaps of the diaphragm substrate are filled with the filling material, the filling material comprises a polymer capable of being dissolved and / or swelled in a lithium ion battery electrolyte, the pre-lithium layer is arranged on one side of the diaphragm substrate, and the protective layer is arranged on the side, away from the diaphragm substrate, of the pre-lithium layer. The method is used for protecting the pre-lithium layer. According to the invention, the filling material is filled in the gap of the diaphragm substrate, so that the diaphragm substrate has a water vapor blocking function, and lithium of the lithium supplementing layer is prevented from being consumed by water vapor before and in the assembly process of the battery; and after the battery is assembled, the polymer is dissolved and swelled in the electrolyte, and gaps of the diaphragm substrate are released to reduce the ionic conductivity of the diaphragm substrate. The technical problems that the ionic conductivity of a diaphragm base body is obviously reduced and the thickness of the diaphragm is increased due to the fact that protective layers are arranged on the upper and lower sides of the diaphragm base body of an existing lithium supplementing diaphragm are solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present disclosure relates to the field of batteries, and in particular, to a pre-lithium composite diaphragm and a preparation method thereof, as well as a lithium ion battery and a preparation method thereof. Background Art

[0002] Lithium-ion batteries have advantages such as high specific energy and long cycle life, and are widely used in electronic products, electric vehicles and other fields. However, existing lithium-ion batteries still have problems such as transition metal dissolution and particle breakage of cathode active materials, which in turn lead to technical problems such as battery cell cycle life attenuation and reduced energy density. In order to alleviate the above technical problems, the prior art proposes to pre-lithiate the anode or cathode to increase the total amount of active lithium during the cycle, which not only helps to improve the battery energy density, but also can significantly extend the service life of the battery cell. However, the existing anode / cathode pre-lithiation has problems such as cumbersome operation, high risk, low utilization rate of metal lithium, high humidity requirements for storage and use environment, and high cost.

[0003] Although there are reports on lithium replenishment on the diaphragm layer, the lithium in the existing lithium replenishment diaphragm is easily consumed by reacting with water, gas, etc. in the air during the assembly process, and the lithium consumption is large, resulting in the inability of the existing lithium replenishment diaphragm for lithium-ion batteries to adapt to the assembly environment of lithium-ion batteries, limiting its industrial application. The existing lithium replenishment diaphragm also sets inorganic materials such as metals and metal compounds on the surface of the diaphragm as a protective layer, which makes the porosity of the diaphragm low, affects the ionic conductivity of the battery cell after assembly, and further affects the performance of the battery cell, and the cost is high. Moreover, setting a protective layer on the upper and lower surfaces of the diaphragm also increases the overall thickness of the diaphragm and reduces the volume energy density of the battery. In addition, the existing construction method of setting a protective layer on the surface of the diaphragm requires a vacuum environment, cannot be produced continuously, has low efficiency, and has a high production cost. In addition, the temperature and humidity of the environment need to be strictly controlled during storage and use, further increasing the manufacturing cost.

[0004] Therefore, how to propose a pre-lithium composite separator, a lithium-ion battery, and a preparation method to solve or at least alleviate at least one of the above technical problems is a problem that needs to be solved urgently. Summary of the invention

[0005] In view of the above technical problems, the present disclosure provides a pre-lithium composite diaphragm, a lithium-ion battery, and a preparation method to solve or at least alleviate at least one technical problem existing in the above pre-lithium composite diaphragm, a lithium-ion battery, and a preparation method.

[0006] According to a specific embodiment of the present disclosure, in a first aspect, the present disclosure provides a pre-lithium composite separator, comprising: A diaphragm matrix having a void therein; A filling material is filled in the gaps of the diaphragm matrix, the filling material includes a polymer, and the polymer can dissolve and / or swell in the electrolyte of the lithium-ion battery; A pre-lithium layer is disposed on one side of the separator substrate; and The protective layer is arranged on a side of the pre-lithium layer away from the diaphragm substrate and is used to protect the pre-lithium layer.

[0007] Optionally, the polymer includes at least one of a water-based polymer and a solvent-based polymer.

[0008] Optionally, the polymer is a solvent-based polymer, the filling material further includes an organic compound, and the organic compound can be dissolved in the electrolyte of the lithium-ion battery.

[0009] Optionally, in the filling material, the mass ratio of the solvent-based polymer to the organic compound is 1:4 to 50:1.

[0010] Optionally, in the filling material, the mass ratio of the solvent-based polymer to the organic compound is 5:1 to 20:1.

[0011] Optionally, the waterborne polymer includes at least one of waterborne polyester, waterborne polyurethane, waterborne polyacrylate, waterborne polymethacrylate, waterborne polycarbonate, waterborne acrylic polymer and waterborne acrylonitrile polymer.

[0012] Optionally, the solvent-based polymer includes at least one of solvent-based polyester, solvent-based polyurethane, solvent-based acrylic resin, solvent-based polymethacrylate, solvent-based polycarbonate, solvent-based acrylic polymer and solvent-based acrylonitrile polymer.

[0013] Optionally, the organic compound includes at least one of ethylene sulfate, propylene sulfate, and methylene methanedisulfonate.

[0014] Optionally, water-based polymers, solvent-based polymers and organic compounds all have a stable electrochemical window at 0-4.5V.

[0015] Optionally, the primary particle sizes of the water-based polymer, the solvent-based polymer and the organic compound are all less than or equal to 300 nm.

[0016] Alternatively, the organic compound can be dissolved in ester solvents and ether solvents.

[0017] Optionally, the melting point of the organic compound is ≥25°C and it is solid at room temperature.

[0018] According to a specific embodiment of the present disclosure, in a second aspect, the present disclosure provides a lithium-ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, and the separator is any pre-lithium composite separator as described above.

[0019] According to a specific embodiment of the present disclosure, in a third aspect, the present disclosure provides a method for preparing any pre-lithium composite separator as described above, comprising the following steps: Step (S1), preparing a coating liquid, wherein the coating liquid includes the filling material; Step (S2), coating the coating liquid on the surface of the diaphragm substrate, allowing the filling material to penetrate into the gaps in the diaphragm substrate, and filling the gaps in the diaphragm substrate after drying; Step (S3), depositing a pre-lithium layer on one side of the separator substrate obtained in step (S2); Step (S4), depositing a protective layer on the surface of the pre-lithium layer away from the separator substrate.

[0020] Optionally, in step (S1), the solid content of the coating liquid is 1%-50%.

[0021] Optionally, in step (S1), the solid content of the coating liquid is 15%-35%.

[0022] Optionally, the filling material includes an aqueous polymer, and step (S1) includes: diluting the aqueous polymer with a solvent to a solid content of 1%-50% to obtain an aqueous polymer solution, an aqueous polymer emulsion or an aqueous polymer suspension, and then obtaining a coating liquid.

[0023] Optionally, the amount of the aqueous polymer used is 1%-100%, and the amount of the solvent used is 0-99% by mass.

[0024] Optionally, based on mass percentage, the amount of the aqueous polymer used is 15%-35%, and the amount of the solvent used is 65%-85%.

[0025] Optionally, the solvent is at least one of water, ethanol, isopropanol and butanone.

[0026] Optionally, the filling material includes a solvent-based polymer, and step (S1) includes: adding an organic solvent to the solvent-based polymer, adjusting the solid content to 1%-50%, the viscosity to less than 1000 cps, and stirring to obtain a coating liquid.

[0027] Optionally, based on mass percentage, the amount of solvent-based polymer used is 1%-99%, and the amount of organic solvent used is 1%-99%.

[0028] Optionally, based on mass percentage, the amount of solvent-based polymer used is 15%-35%, and the amount of organic solvent used is 65%-85%.

[0029] Optionally, the filling material includes a solvent-based polymer and an organic compound, and step (S1) includes: adding the organic compound to the solvent-based polymer, stirring at a speed of 500-3000 rpm for 10-30 minutes; then adding an organic solvent to adjust the solid content to 1%-50% and the viscosity to less than 1000 cps; and finally stirring to obtain a coating liquid.

[0030] Optionally, based on mass percentage, the amount of solvent-based polymer is 1%-79%, the amount of organic compound is greater than 0 and less than or equal to 20%, and the amount of organic solvent is 1%-99%.

[0031] Optionally, in terms of mass percentage, the amount of the solvent-based polymer is 15% to 35%, the amount of the organic compound is 0.5% to 8%, and the amount of the organic solvent is 57% to 84.5%.

[0032] Optionally, the organic solvent includes at least one of cyclohexane, ethyl acetate, butyl acetate, butanone and pyrrolidone.

[0033] Optionally, in step (S2), the method of coating the coating liquid on the surface of the diaphragm substrate is wet coating, including at least one of dip coating, roller coating, spray coating, spin coating, blade coating and transfer coating.

[0034] Optionally, the wet coating amount of the coating liquid on the surface of the diaphragm substrate is 1-10 g / m 2 , coating speed is 0-150mpm, and drying temperature is 60-110℃.

[0035] Optionally, the wet coating amount of the coating liquid on the surface of the diaphragm substrate is 3-5 g / m 2 , coating speed is 100-120mpm, and drying temperature is 60-75℃.

[0036] According to a specific embodiment of the present disclosure, in a fourth aspect, the present disclosure provides a method for preparing a lithium ion battery, comprising the following steps: Evenly coating the positive electrode active material on the surface of the positive electrode current collector to form a positive electrode sheet; Evenly coating the negative electrode active material on the surface of the negative electrode current collector to form a negative electrode sheet; A pre-lithium composite diaphragm is prepared by any of the above-mentioned methods for preparing a pre-lithium composite diaphragm; The pre-lithium composite diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet, the pre-lithium composite diaphragm and the negative electrode sheet are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.

[0037] Compared with the prior art, the above solution of the embodiment of the present disclosure has at least the following beneficial effects: (1) The pre-lithium composite diaphragm provided by the present disclosure fills the gaps of the diaphragm matrix with a filling material including a polymer, which can extend the path for water vapor and the like to pass through the diaphragm, so that the diaphragm matrix has a barrier function for water vapor and the like, and can protect the pre-lithium layer, thereby preventing the lithium of the lithium replenishment diaphragm from being consumed by water, gas, etc. in the air before and during battery assembly, thereby affecting the lithium replenishment efficiency; and the polymer can dissolve and / or swell in the electrolyte of the lithium-ion battery. After the battery is assembled, the polymer can dissolve and / or swell in the electrolyte, releasing the gaps of the diaphragm matrix to restore the ionic conductivity of the diaphragm matrix, thereby avoiding the technical problem that the protective layer of the existing lithium replenishment diaphragm significantly reduces the ionic conductivity of the diaphragm matrix. Moreover, the polymer only physically dissolves and swells in the electrolyte, without chemical reaction, and has no effect on the electrolyte and the diaphragm.

[0038] (2) The pre-lithium composite diaphragm disclosed in the present invention is a diaphragm matrix with a polymer filled in the voids. No protective layer is provided on the surface of the diaphragm matrix, which does not increase the thickness of the diaphragm matrix and is beneficial for maintaining or even improving the volume energy density of lithium-ion batteries. Moreover, after the voids are filled with the filling material, the vapor-deposited lithium metal can be prevented from entering the voids of the diaphragm matrix during the formation of the pre-lithium layer, thereby affecting the air permeability of the lithium-supplementing diaphragm.

[0039] (3) The filling material disclosed in the present invention can be directly produced continuously by coating in an open environment, without the need for vacuum evaporation through a vacuum coating machine, thereby minimizing the time cost of equipment evacuation, vacuum breaking, equipment cleaning, etc., thereby reducing process difficulty and improving production efficiency; and there is no need to strictly control the temperature and humidity of the environment, which can further reduce manufacturing costs.

[0040] (4) The filling material disclosed in the present invention is organic and has a lower cost than the existing metal or metal alloy protective layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] The drawings herein are incorporated into the specification and constitute a part of the specification, showing embodiments consistent with the present disclosure, and together with the specification, are used to explain the principles of the present disclosure. Obviously, the drawings described below are only some embodiments of the present disclosure, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without creative work. In the drawings: Figure 1 It is a schematic diagram of the structure of the pre-lithium composite diaphragm in the embodiment of the present disclosure; Figure 2 Schematic diagram of the cell structure of a lithium-ion battery in an embodiment of the present disclosure; Figure 3 A flow chart of a method for preparing a lithium-supplementing diaphragm for a lithium-ion battery provided in an embodiment of the present disclosure; Figure 4A flow chart of a method for preparing a lithium-ion battery provided in an embodiment of the present disclosure; Figure 5 This is a transmission electron microscope (TEM) photograph of the uncoated alumina ceramic coating diaphragm in Comparative Example 1 of the present disclosure; Figure 6 This is a transmission electron microscope (TEM) photograph of the alumina ceramic coating diaphragm after the coating liquid is coated on the surface of the alumina ceramic coating diaphragm substrate and dried according to Example 6 of the present disclosure.

[0042] The reference numerals in the specific implementation manner are as follows: Lithium ion battery 100; A pre-lithium composite separator 10 , a separator substrate 1 , a filling material 2 , a pre-lithium layer 3 , a protective layer 4 , a positive electrode sheet 20 , and a negative electrode sheet 30 . DETAILED DESCRIPTION

[0043] In order to make the purpose, technical solutions and advantages of the present disclosure clearer, the present disclosure will be further described in detail below in conjunction with the accompanying drawings. Obviously, the described embodiments are only part of the embodiments of the present disclosure, rather than all of the embodiments. Based on the embodiments in the present disclosure, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present disclosure.

[0044] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as commonly understood by one of ordinary skill in the art to which the present disclosure belongs; the terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the present disclosure.

[0045] It should also be noted that the terms "include", "comprises" or any other variations thereof are intended to cover non-exclusive inclusion, so that a product or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such product or device. In the absence of more restrictions, the elements defined by the sentence "comprises a" do not exclude the presence of other identical elements in the product or device including the elements.

[0046] In the description of the embodiments of the present disclosure, the orientation or positional relationship indicated by the technical terms "upper", "lower", "thickness", etc. is based on the orientation or positional relationship shown in the accompanying drawings, and is only for the convenience of describing the embodiments of the present disclosure and simplifying the description, rather than indicating or implying that the referred device or element must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the embodiments of the present disclosure.

[0047] In the description of the embodiments of the present disclosure, the term "and / or" is used only to describe the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. In addition, the character " / " in this article generally indicates that the associated objects before and after are in an "or" relationship.

[0048] In the description of the embodiments of the present disclosure, the symbol “-” represents the two endpoint data before and after the “-” and all data between the two endpoints. For example, AB represents all data greater than or equal to A and less than or equal to B.

[0049] Reference to "embodiments" in this disclosure means that a particular feature, structure, or characteristic described in conjunction with the embodiments may be included in at least one embodiment of the disclosure. The appearance of the phrase in various places in the specification does not necessarily refer to the same embodiment, nor is it an independent or alternative embodiment that is mutually exclusive with other embodiments. It is explicitly and implicitly understood by those skilled in the art that the embodiments described in this disclosure may be combined with other embodiments.

[0050] Most of the existing lithium-ion battery lithium replenishment methods are achieved through anode / cathode pre-lithiation technology. However, the existing anode / cathode pre-lithiation has technical problems such as cumbersome operation, high risk, low utilization rate of metal lithium, and high cost. After research, the inventors found that diaphragm pre-lithiation can also increase the total amount of active lithium during the battery cycle, which not only helps to improve the battery energy density, but also can significantly extend the service life of the battery cell.

[0051] However, the inventors have also found through research that the lithium in the existing lithium-supplementing diaphragm is easily consumed by reacting with water, gas, etc. in the air during the assembly process, and the lithium consumption is large, which causes the existing lithium-ion battery lithium-supplementing diaphragm to be unable to adapt to the assembly environment of lithium-ion batteries, limiting its industrial application. The existing lithium-supplementing diaphragm also sets inorganic materials such as metals and metal compounds on the surface of the diaphragm as a protective layer, so that the porosity of the diaphragm is relatively low, which affects the ionic conductivity of the battery cell after assembly, and further affects the performance of the battery cell, and the cost is relatively high. Moreover, setting a protective layer on the upper and lower surfaces of the diaphragm also increases the overall thickness of the diaphragm and reduces the volume energy density of the battery. The existing construction method of setting a protective layer on the surface of the diaphragm requires a vacuum environment, cannot be produced continuously, has low efficiency, and has a high production cost. In addition, the temperature and humidity of the environment need to be strictly controlled during storage and use, further increasing the manufacturing cost. In addition, in the process of forming the pre-lithium layer of the existing lithium-supplementing diaphragm, the evaporated lithium metal easily enters the diaphragm gap, affecting the air permeability of the diaphragm.

[0052] In order to solve or at least alleviate the above-mentioned technical problems, the present invention fills the voids in the diaphragm matrix with filling material so that the diaphragm matrix has a water vapor barrier function, which can protect the pre-lithium layer, thereby preventing the lithium of the lithium-replenishing diaphragm from being consumed by water and gas in the air before and during battery assembly, thereby affecting the lithium replenishment efficiency; and the filling material includes a polymer, and the polymer can dissolve and / or swell in the electrolyte of the lithium-ion battery. After the battery is assembled, the polymer can dissolve and / or swell in the electrolyte, releasing the voids in the diaphragm matrix to restore the ionic conductivity of the diaphragm matrix.

[0053] Specifically, the present disclosure provides a pre-lithium composite separator, comprising: A diaphragm matrix having a void therein; A filling material is filled in the gaps of the diaphragm matrix, the filling material includes a polymer, and the polymer can dissolve and / or swell in the electrolyte of the lithium-ion battery; A pre-lithium layer is disposed on one side of the separator substrate; and The protective layer is arranged on a side of the pre-lithium layer away from the diaphragm substrate and is used to protect the pre-lithium layer.

[0054] The present disclosure also provides a method for preparing the above-mentioned pre-lithium composite diaphragm, comprising the following steps: Step (S1), preparing a coating liquid, wherein the coating liquid includes the filling material; Step (S2), coating the coating liquid on the surface of the diaphragm substrate, allowing the filling material to penetrate into the gaps in the diaphragm substrate, and filling the gaps in the diaphragm substrate after drying; Step (S3), depositing a pre-lithium layer on one side of the separator substrate obtained in step (S2); Step (S4), depositing a protective layer on the surface of the pre-lithium layer away from the separator substrate.

[0055] In the technical solution disclosed in the present invention, a filling material including a polymer is filled in the voids of the diaphragm matrix, which can extend the path of water vapor passing through the diaphragm, so that the diaphragm matrix has a water and gas barrier function, and can protect the pre-lithium layer, thereby avoiding the lithium of the lithium-supplementing diaphragm being consumed by water and gas in the air before and during the assembly of the battery, affecting the lithium replenishment efficiency; and the polymer can dissolve and / or swell in the electrolyte of the lithium-ion battery. After the battery is assembled, the polymer can dissolve and / or swell in the electrolyte, releasing the voids of the diaphragm matrix to restore the ionic conductivity of the diaphragm matrix, avoiding the technical problem that the protective layer of the existing lithium-supplementing diaphragm significantly reduces the ionic conductivity of the diaphragm matrix. Moreover, the polymer only physically dissolves and swells in the electrolyte, without chemical reaction, and has no effect on the electrolyte and the diaphragm. Filling the polymer in the voids of the diaphragm matrix disclosed in the present invention will not increase the thickness of the diaphragm matrix, which is conducive to maintaining or even improving the volume energy density of the lithium-ion battery; and it can also avoid the vapor-deposited lithium metal entering the voids of the diaphragm matrix in the process of forming the pre-lithium layer, affecting the permeability of the lithium-supplementing diaphragm. The filling material disclosed in the present invention can be directly produced in an open environment by coating, without the need for vacuum evaporation by a vacuum coating machine, which minimizes the time cost of equipment vacuuming, vacuum breaking, equipment cleaning, etc., thereby improving production efficiency; and there is no need to strictly control the temperature and humidity of the environment, which can further reduce the manufacturing cost. The filling material disclosed in the present invention is an organic matter, which is lower in cost than the existing metal and metal alloy protective layers.

[0056] The optional embodiments of the present disclosure are described in detail below with reference to the accompanying drawings.

[0057] See also Figure 1 The first embodiment of the present disclosure provides a pre-lithium composite diaphragm 10, comprising: a diaphragm substrate 1, a filling material 2, a pre-lithium layer 3 and a protective layer 4. The filling material 2 is filled in the gap of the diaphragm substrate 1, the pre-lithium layer 3 is arranged on one side of the diaphragm substrate 1, and the protective layer 4 is arranged on the side of the pre-lithium layer 3 away from the diaphragm substrate 1.

[0058] The diaphragm matrix 1 can be a conventional diaphragm of a lithium ion battery. As an example, the diaphragm matrix 1 can include but is not limited to a base film, a base film / ceramic composite diaphragm, a base film / adhesive composite diaphragm or a base film / ceramic / adhesive composite diaphragm. The base film includes but is not limited to a polyethylene base film, a polyethylene non-woven base film, a polypropylene base film, a polypropylene non-woven base film, a polypropylene / polyethylene / polypropylene composite base film, a polyimide base film, a polyimide non-woven base film, a polytetrafluoroethylene-based film, a polytetrafluoroethylene non-woven base film, a polyvinyl chloride-based film and a polyvinyl chloride non-woven base film. Ceramics include but are not limited to at least one of aluminum oxide, zirconium oxide, boehmite, magnesium hydroxide, barium sulfate, silicon oxide, aluminum nitride, magnesium oxide, titanium dioxide, yttrium oxide and cerium oxide. Adhesives include but are not limited to at least one of polytetrafluoroethylene, polyvinylidene fluoride, acrylic acid, polyethylene oxide, sodium carboxymethyl cellulose, styrene-butadiene rubber, hydroxypropyl methylcellulose, carboxystyrene-butadiene latex and polyvinyl alcohol. The thickness of the diaphragm substrate 1 is preferably, but not limited to, 5-50 μm. In this embodiment, the thickness of the diaphragm substrate 1 is 13 μm, etc.

[0059] The filling material 2 is capable of dissolving and / or swelling in the electrolyte of the lithium-ion battery. The filling material 2 includes a polymer, and the polymer is capable of dissolving and / or swelling in the electrolyte of the lithium-ion battery. The polymer may include at least one of a water-based polymer and a solvent-based polymer. In some embodiments, the polymer is a water-based polymer; in some embodiments, the polymer is a solvent-based polymer; in other embodiments, the polymer includes a water-based polymer and a solvent-based polymer.

[0060] The aqueous polymer has a stable electrochemical window at 0-4.5V, which prevents the aqueous polymer from participating in the battery reaction during the battery charge and discharge process, resulting in deterioration of battery stability. The aqueous polymer can be dissolved in the electrolyte at room temperature. The primary particle size of the aqueous polymer is preferably ≤300nm, and it can enter the gap of the diaphragm matrix 1. The aqueous polymer includes but is not limited to at least one of aqueous polyester, aqueous polyurethane, aqueous polyacrylate, aqueous polymethacrylate, aqueous polycarbonate, aqueous acrylic polymer and aqueous acrylonitrile polymer.

[0061] The solvent-based polymer has a stable electrochemical window at 0-4.5V, which prevents the solvent-based polymer from participating in the battery reaction during the battery charge and discharge process, resulting in deterioration of battery stability. The solvent-based polymer can be dissolved in the electrolyte at room temperature. The primary particle size of the solvent-based polymer is preferably ≤300nm, and can enter the gap of the diaphragm matrix 1. The solvent-based polymer includes but is not limited to at least one of solvent-based polyester, solvent-based polyurethane, solvent-based acrylic resin, solvent-based polymethacrylate, solvent-based polycarbonate, solvent-based acrylic polymer and solvent-based acrylonitrile polymer.

[0062] In some embodiments, the filler material 2 includes the solvent-based polymer and an organic compound, and the organic compound can be dissolved in the electrolyte of the lithium-ion battery. In some embodiments, the mass ratio of the solvent-based polymer to the organic compound is 1:4 to 50:1. In some preferred embodiments, the mass ratio of the solvent-based polymer to the organic compound is 5:1 to 20:1.

[0063] The organic compound is preferably soluble in ester solvents and ether solvents. The organic compound has a stable electrochemical window at 0-4.5V to avoid the organic compound participating in the battery reaction during the battery charge and discharge process, resulting in deterioration of battery stability. The melting point of the organic compound is ≥25°C, and it is solid at room temperature. After drying, it fills the diaphragm gap together with the solvent-based polymer. After assembly, it can be dissolved in the electrolyte to form a gap and provide an ion channel. The organic compound includes but is not limited to at least one of ethylene sulfate, propylene sulfate, and methylene disulfonate.

[0064] The organic compound has a small molecular weight, high solubility in the electrolyte, fast dissolution rate, and can release the diaphragm gap faster. In addition, the organic compound is a common auxiliary agent for the electrolyte, which can improve the low-temperature performance of the electrolyte.

[0065] The lithium supplement layer 3 can compensate for the irreversible lithium loss of the lithium-ion battery during the first charge and discharge and cycle process, thereby improving the capacity and energy density of the battery. The material of the pre-lithium layer 3 can be but is not limited to metallic lithium, lithium silicon alloy, lithium magnesium alloy, lithium copper alloy, lithium silver alloy, lithium beryllium alloy, lithium zinc alloy, lithium cadmium alloy, lithium aluminum alloy, lithium gold alloy and lithium boron alloy. The thickness of the pre-lithium layer 3 is preferably but not limited to 0.1-10µm. In this embodiment, the thickness of the pre-lithium layer 3 is 1µm.

[0066] The protective layer 4 is used to protect the pre-lithium layer 3, preventing the lithium in the pre-lithium layer 3 from being directly exposed to the air and being consumed by water and gas in the air during the assembly of the battery cell. The protective layer 4 is preferably made of a material with high ionic conductivity. While providing protection for the pre-lithium layer 3, it can improve the overall ionic conductivity of the pre-lithium composite diaphragm 10 and improve the efficiency and effect of lithium replenishment during its use. In some embodiments, the protective layer 4 is an inorganic protective layer. The materials of the protective layer 4 include but are not limited to Al2O3, MgO, ZnO2, TiO2, ZrO2, LaO2, CeO2, Y2O3, Si x O, SiC, SiN x 、SiCN x , AlN, Mg(OH)2, BaSO4, boehmite or perovskite; or, Li2CO3, Li3N, LiF, Li3PO4, Li4SiO4, Li4Ti5O 12At least one of LiPON, LiSiON, LLZO, LLZTO, LATP, Li3Fe2(PO4)3, Li3V2(PO4)3, Li3In2(PO4)3, Li3Sc2(PO4)3, and Li3Cr2(PO4)3. The thickness of the protective layer 4 is preferably, but not limited to, 10-1000 nm. In this embodiment, the thickness of the protective layer 4 is 30 nm.

[0067] The present disclosure also provides a lithium-ion battery 100. Figure 2 It is a schematic diagram of the cell structure of a lithium-ion battery 100 , including: the pre-lithium composite separator 10 , a positive electrode sheet 20 and a negative electrode sheet 30 , wherein the pre-lithium composite separator 10 is located between the positive electrode sheet 20 and the negative electrode sheet 30 .

[0068] See also Figure 3 The present disclosure also provides a method for preparing any of the above-mentioned pre-lithium composite separators 10, comprising the following steps: Step (S1), preparing a coating liquid, wherein the coating liquid includes the filling material 2; Step (S2), coating the coating liquid on the surface of the diaphragm substrate 1, allowing the filling material 2 to penetrate into the gaps in the diaphragm substrate 1, and filling the gaps in the diaphragm substrate 1 after drying; Step (S3), depositing the pre-lithium layer 3 on one side of the diaphragm substrate 1 obtained in step (S2); Step (S4), depositing the protective layer 4 on the surface of the pre-lithium layer 3 away from the diaphragm substrate 1.

[0069] In step (S1), the solid content of the coating liquid may be 1%-50%. In some preferred embodiments, the solid content of the coating liquid is 15%-35%.

[0070] In some embodiments, the filling material 2 includes the aqueous polymer, and the method for preparing the coating liquid includes: diluting the aqueous polymer to a solid content of 1%-50% with a solvent to obtain an aqueous polymer solution, an aqueous polymer emulsion or an aqueous polymer suspension, and then obtaining the coating liquid. Since the aqueous polymer can be liquid or solid, the amount of the aqueous polymer can be 1%-100% by mass percentage, and the amount of the solvent can be 0-99%. Preferably, the amount of the aqueous polymer is 15%-35% by mass percentage, and the amount of the solvent is 65%-85%. The solvent is preferably, but not limited to, one or more of water, ethanol, isopropanol and butanone.

[0071] In some embodiments, the filling material 2 includes the solvent-based polymer, and step (S1) includes: adding an organic solvent to the solvent-based polymer, adjusting the solid content to 1%-50%, the viscosity to less than 1000cps, and stirring to obtain the coating liquid. Wherein, in terms of mass percentage, the amount of the solvent-based polymer can be 1%-99%, and the amount of the organic solvent can be 1%-99%. Preferably, in terms of mass percentage, the amount of the solvent-based polymer is 15%-35%, and the amount of the organic solvent is 65%-85%.

[0072] In other embodiments, the filling material 2 includes the solvent-based polymer and the organic compound, and step (S1) includes: adding the organic compound to the solvent-based polymer, stirring at a speed of 500-3000 rpm for 10-30 minutes; then adding an organic solvent to adjust the solid content to 1%-50% and the viscosity to less than 1000 cps; finally, stirring to obtain the coating liquid. Wherein, in terms of mass percentage, the amount of the solvent-based polymer can be 1%-79%, the amount of the organic compound can be greater than 0 and less than or equal to 20%, and the amount of the organic solvent can be 1%-99%. Preferably, in terms of mass percentage, the amount of the solvent-based polymer is 15%~35%, the amount of the organic compound is 0.5%~8%, and the amount of the organic solvent is 57%~84.5%. The organic solvent includes but is not limited to a mixture of one or more of cyclohexane, ethyl acetate, butyl acetate, butanone and pyrrolidone.

[0073] In step (S2), the method of coating the coating liquid on the surface of the membrane substrate 1 includes, but is not limited to, wet coating such as dip coating, roller coating, spray coating, spin coating, blade coating, transfer coating, etc. Roll coating or spray coating is preferably used. In some embodiments, the wet coating amount of the coating liquid on the surface of the membrane substrate 1 is 1-10 g / m 2 , the coating speed is 0-150mpm, and the drying temperature is 60-110°C. In some preferred embodiments, the wet coating amount of the coating liquid on the surface of the membrane substrate 1 is 3-5g / m 2 , coating speed is 100-120mpm, and drying temperature is 60-75℃.

[0074] The membrane substrate obtained in step (S2) after coating and drying is rolled up for use. The water vapor barrier performance of the membrane substrate obtained in step (S2) can also be tested to determine the water vapor barrier performance of the pre-lithium composite membrane 10 obtained by the preparation method before and during battery assembly.

[0075] In step (S3), the pre-lithium layer 3 is deposited on one side of the diaphragm substrate 1 obtained in step (S2) by methods including but not limited to vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering. In this embodiment, the pre-lithium layer 3 is deposited on one side of the diaphragm substrate 1 obtained in step (S2) by vacuum evaporation.

[0076] Step (S4), the method of depositing the protective layer 4 on the surface of the pre-lithium layer 3 away from the diaphragm substrate 1 includes but is not limited to scraping, roller coating, spraying, chemical vapor deposition, plasma vapor deposition, atomic layer deposition, pulsed laser deposition, vacuum evaporation, ion plating, radio frequency sputtering, magnetron sputtering or reactive sputtering, etc. In this embodiment, the protective layer 4 is deposited on the surface of the pre-lithium layer 3 away from the diaphragm substrate 1 by vacuum evaporation process.

[0077] See also Figure 4 The present disclosure also provides a method for preparing a lithium-ion battery, comprising the following steps: Evenly coating the positive electrode active material on the surface of the positive electrode current collector to form a positive electrode sheet; Evenly coating the negative electrode active material on the surface of the negative electrode current collector to form a negative electrode sheet; The pre-lithium composite diaphragm 10 is obtained by using any of the methods for preparing the pre-lithium composite diaphragm described in the above embodiments; The pre-lithium composite separator 10 is disposed between the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet, the pre-lithium composite separator and the negative electrode sheet are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.

[0078] The positive electrode collector, positive electrode active material, negative electrode collector, negative electrode active material, shell and electrolyte can be selected from the positive electrode collector, positive electrode active material, negative electrode collector, negative electrode active material, shell and electrolyte commonly used in lithium ion batteries.

[0079] The preparation process, test methods and test data of the embodiments and comparative examples are introduced below: Example

[0080] The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, and the gaps in the 13µm alumina ceramic coating diaphragm substrate are filled with waterborne polyurethane. The preparation method comprises the following steps: Step (S1), diluting the water-based polyurethane to a solid content of 15% with water and ethanol to obtain a coating solution, wherein the water-based polyurethane: water: ethanol = 50%: 20%: 30%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 5g / m 2, dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium metal layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the lithium metal layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3. Example

[0081] The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, the voids of the 13µm alumina ceramic coating diaphragm substrate are filled with water-based polyester and water-based polyacrylate, and the preparation method comprises the following steps: Step (S1), diluting the water-based polyester and the water-based polyacrylate with water and isopropanol to a solid content of 5% to obtain a coating solution, wherein the water-based polyester: water-based polyacrylate: water: isopropanol = 15%: 30%: 45%: 10%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 10g / m 2 , dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium-magnesium alloy layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the pre-lithium layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3. Example

[0082] The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, and the gaps in the 13µm alumina ceramic coating diaphragm substrate are filled with water-based polymethyl methacrylate and water-based polycarbonate. The preparation method comprises the following steps: Step (S1), diluting water-based polymethyl methacrylate and water-based polycarbonate with water and butanone to a solid content of 20% to obtain a coating solution, wherein the water-based polymethyl methacrylate: water-based polycarbonate: water: butanone = 10%: 10%: 55%: 25%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 1g / m 2 , dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium aluminum alloy layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the pre-lithium layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3.

[0083] Embodiment 4: The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, the voids of the 13µm alumina ceramic coating diaphragm substrate are filled with solvent-based polyurethane and ethylene sulfate, and the preparation method comprises the following steps: Step (S1), using cyclohexane and butyl acetate to dilute the solvent-based polyurethane and ethylene sulfate to a solid content of 35%, to obtain a coating solution, wherein the solvent-based polyurethane: ethylene sulfate: cyclohexane: butyl acetate = 5%: 1%: 45%: 49%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 2g / m 2 , dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium metal layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the pre-lithium layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3.

[0084] Embodiment 5: The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, the voids of the 13µm alumina ceramic coating diaphragm substrate are filled with solvent-based polyester and methylene disulfonate, and the preparation method comprises the following steps: Step (S1), using cyclohexane and butyl acetate to dilute the solvent-based polyurethane and ethylene sulfate to a solid content of 18%, to obtain a coating solution, wherein the solvent-based polyester: methylene methane disulfonate: butyl acetate = 50%: 15%: 35%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 10g / m 2 , dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium-silicon alloy layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the pre-lithium layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3.

[0085] Embodiment 6: The pre-lithium composite diaphragm of this embodiment comprises: a 13µm alumina ceramic coating diaphragm substrate, a 1µm pre-lithium layer and a 30nm Li2CO3 protective layer, the voids of the 13µm alumina ceramic coating diaphragm substrate are filled with solvent-based polymethyl methacrylate, propylene sulfate and propylene carbonate, and the preparation method comprises the following steps: Step (S1), using ethyl acetate to dilute solvent-based polymethyl methacrylate, solvent-based propylene sulfate and solvent-based propylene carbonate to a solid content of 15% to obtain a coating solution, wherein solvent-based polymethyl methacrylate: propylene sulfate: propylene carbonate: ethyl acetate = 35%: 10%: 15%: 40%; Step (S2), coating the coating liquid on the surface of the alumina ceramic coating diaphragm substrate, with a wet coating amount of 8g / m 2 , dry and roll for use, and test its water vapor barrier performance; Step (S3), depositing a 1µm lithium-zinc alloy layer as a pre-lithium layer on the upper surface of the alumina ceramic coating diaphragm substrate by vacuum evaporation process; Step (S4), depositing a 30nm protective layer on the upper surface of the pre-lithium layer by vacuum evaporation technology, wherein the component of the protective layer is Li2CO3.

[0086] Comparative Example 1: The diaphragm is made of untreated 13µm alumina ceramic coating.

[0087] The water vapor barrier performance of the membrane substrate after coating and drying in step (S2) of Examples 1-6 and the membrane of Comparative Example 1 was tested using a water vapor transmission rate tester, wherein the test temperature was 23° C. and the relative humidity was 10% RH. The test data is shown in Table 1.

[0088] Assemble button-type half-cells, use stainless steel for the positive electrode and the negative electrode, use HR9212 for the electrolyte, and use the pre-lithium composite diaphragms obtained in Examples 1-6 and the diaphragm of Comparative Example 1 for the diaphragm. After standing at room temperature for 48 hours, the ionic conductivity of the diaphragm is tested, and the test data is shown in Table 1.

[0089] It can be seen from Table 1 that the water vapor barrier performance of the diaphragms in Examples 1-6 is much better than that of the existing diaphragm in Comparative Example 1; the ionic conductivity of the diaphragms in Examples 1-6 is not much different from that of the diaphragm in Comparative Example 1. The above results show that the present disclosure fills the gaps in the diaphragm matrix with a filling material including a polymer, which can well improve the water vapor barrier performance of the diaphragm; and because the filling material of the present disclosure can dissolve and / or swell in the electrolyte, the pre-lithium composite diaphragm of the present disclosure has little effect on the ionic conductivity, and while replenishing lithium and enhancing the water vapor barrier, the ionic conductivity of the pre-lithium diaphragm will not be significantly reduced.

[0090] It can also be seen from Table 1 that the lithium consumption of the diaphragms in Examples 1-6 is much lower than that of the diaphragm in Comparative Example 1, indicating that the present invention fills the voids in the diaphragm matrix with a filling material including a polymer, which can better protect the pre-lithium layer, greatly reduce the lithium consumption of the pre-lithium layer, and improve the utilization rate of lithium.

[0091] See also Figure 5 , is a transmission electron microscope (TEM) photograph of the alumina ceramic coating diaphragm without coating in Comparative Example 1 of the present disclosure, Figure 5 As can be seen, there are many voids in the diaphragm. Figure 6 , is a transmission electron microscope (TEM) photograph of the alumina ceramic coating diaphragm after the coating liquid is applied to the surface of the alumina ceramic coating diaphragm substrate in Example 6 of the present disclosure and dried, from Figure 6 It can be seen that the gaps in the alumina ceramic coating diaphragm substrate are basically filled with filling materials, and the surface of the alumina ceramic coating diaphragm substrate is flat after treatment. This shows that the coating method disclosed in the present invention can fill the gaps in the diaphragm substrate with filling materials, thereby making the diaphragm substrate have a water vapor barrier function, which can protect the pre-lithium layer and prevent the lithium of the lithium replenishing diaphragm from being consumed by water and gas in the air before and during battery assembly, thereby affecting the lithium replenishment efficiency.

[0092] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present disclosure, rather than to limit them; although the present disclosure has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein by equivalents; and these modifications or replacements do not make the essence of the corresponding technical solutions deviate from the scope of the technical solutions of the embodiments of the present disclosure, and they should all be included in the scope of the claims and specification of the present disclosure. In particular, as long as there is no structural conflict, the various technical features mentioned in the various embodiments can be combined in any way. The present disclosure is not limited to the specific embodiments disclosed herein, but includes all technical solutions that fall within the scope of the claims.

Claims

1. A pre-lithium composite diaphragm, characterized in that: include: A diaphragm substrate having a void therein; A filling material, wherein the filling material is filled in the voids of the diaphragm matrix, the filling material comprises a polymer, and the polymer can be dissolved and / or swelled in the electrolyte of the lithium ion battery; A pre-lithium layer is arranged on one side of the separator substrate; as well as The protective layer is arranged on a side of the pre-lithium layer away from the diaphragm substrate and is used to protect the pre-lithium layer.

2. The pre-lithium composite diaphragm according to claim 1, characterized in that: The polymer includes at least one of a water-based polymer and a solvent-based polymer.

3. The pre-lithium composite diaphragm according to claim 2, characterized in that: The polymer is a solvent-based polymer, and the filling material further includes an organic compound, and the organic compound can be dissolved in the electrolyte of the lithium-ion battery.

4. The pre-lithium composite diaphragm according to claim 3, characterized in that: In the filling material, the mass ratio of the solvent-based polymer to the organic compound is 1:4 to 50:

1.

5. The pre-lithium composite separator according to any one of claims 2 to 4, characterized in that: The waterborne polymer comprises: at least one of waterborne polyester, waterborne polyurethane, waterborne polyacrylate, waterborne polymethacrylate, waterborne polycarbonate, waterborne acrylic polymer and waterborne acrylonitrile polymer; And / or, the solvent-based polymer includes at least one of solvent-based polyester, solvent-based polyurethane, solvent-based acrylic resin, solvent-based polymethacrylate, solvent-based polycarbonate, solvent-based acrylic polymer and solvent-based acrylonitrile polymer; And / or, the organic compound includes at least one of ethylene sulfate, propylene sulfate, and methylene methanedisulfonate.

6. The pre-lithium composite separator according to any one of claims 1 to 4, characterized in that: The water-based polymer, the solvent-based polymer and the organic compound all have a stable electrochemical window at 0-4.5V; And / or, the primary particle sizes of the water-based polymer, the solvent-based polymer and the organic compound are all less than or equal to 300 nm.

7. A lithium ion battery, comprising a positive electrode sheet, a negative electrode sheet and a separator, wherein the separator is located between the positive electrode sheet and the negative electrode sheet, characterized in that: The separator is a pre-lithium composite separator as described in any one of claims 1 to 6.

8. A method for preparing a pre-lithium composite diaphragm according to any one of claims 1 to 6, characterized in that: The following steps are involved: Step (S1), preparing a coating liquid, wherein the coating liquid includes the filling material; Step (S2), coating the coating liquid on the surface of the diaphragm substrate, allowing the filling material to penetrate into the gaps in the diaphragm substrate, and filling the gaps in the diaphragm substrate after drying; Step (S3), depositing the pre-lithium layer on one side of the separator substrate obtained in step (S2); Step (S4), depositing the protective layer on the surface of the pre-lithium layer away from the diaphragm substrate.

9. The method for preparing the pre-lithium composite diaphragm according to claim 8, characterized in that: The filling material includes the aqueous polymer, and the step (S1) includes: using a solvent to dilute the aqueous polymer to a solid content of 1%-50% to obtain an aqueous polymer solution, an aqueous polymer emulsion or an aqueous polymer suspension, and then obtaining the coating liquid; And / or, the filling material includes the solvent-based polymer, and the step (S1) includes: adding an organic solvent to the solvent-based polymer, adjusting the solid content to 1%-50%, the viscosity to less than 1000 cps, and stirring to obtain the coating solution; And / or, the filling material includes the solvent-based polymer and the organic compound, and the step (S1) includes: adding the organic compound to the solvent-based polymer, stirring at a speed of 500-3000 rpm for 10-30 minutes; then adding an organic solvent to adjust the solid content to 1%-50% and the viscosity to less than 1000 cps; finally, stirring to obtain the coating liquid.

10. A method for preparing a lithium ion battery, characterized in that: The following steps are involved: Evenly coating the positive electrode active material on the surface of the positive electrode current collector to form a positive electrode sheet; Evenly coating the negative electrode active material on the surface of the negative electrode current collector to form a negative electrode sheet; The pre-lithium composite diaphragm is prepared by the method for preparing the pre-lithium composite diaphragm according to claim 8 or 9; The pre-lithium composite diaphragm is arranged between the positive electrode sheet and the negative electrode sheet, and the positive electrode sheet, the pre-lithium composite diaphragm and the negative electrode sheet are placed in a shell, and the shell is sealed after the electrolyte is injected into the shell.

Citation Information

Patent Citations

  • Solid electrolyte membrane of lithium battery as well as preparation method and application of solid electrolyte membrane

    CN107275673A

  • Multilayer structure composite diaphragm, preparation method thereof, secondary battery and electric equipment

    CN112886143A

  • Lithium metal battery diaphragm as well as preparation method and application thereof

    CN114843705A

  • Current collector and preparation method and application thereof

    CN117936805A

  • Separator for lithium secondary battery, manufacturing method therefor, and lithium secondary battery including same