Preparation method and application of stretchable transparent composite electrode and solar cell

By using silver nanowires and sulfonimide salt-modified PH1000 film in transparent electrodes of organic solar cells, combined with oxygen plasma treatment and water vapor annealing, it is solved that it is difficult to achieve high performance and tensile properties in the prior art. The problem has achieved efficient photoelectric energy conversion and improved mechanical performance.

CN118984639APending Publication Date: 2024-11-19ZHEJIANG UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411064349.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-05
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

Existing research is difficult to achieve high performance and good tensile properties of organic solar cells without sacrificing photoelectric properties, especially the development of stretchable transparent electrodes.

Method used

By spin-coating silver nanowires (AgNWs) dispersion on a stretchable substrate and annealing on a water vapor layer, an AgNWs film was formed, and then coated with a sulfonimide salt-modified PH1000 solution on the AgNWs film. A composite electrode with high elongation, high light transmittance and high conductivity was prepared by combining oxygen plasma treatment and dropwise addition of sulfonimide salt solution.

Benefits of technology

A composite electrode that maintains high conductivity under high tensile conditions is realized, which improves the photoelectric energy conversion efficiency of solar cells and enhances the mechanical properties and light transmittance of the electrodes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984639A_ABST
    Figure CN118984639A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a stretchable transparent composite electrode, and the preparation method comprises the steps: carrying out the first oxygen plasma treatment and steam annealing of a stretchable substrate, thereby forming a steam layer on the stretchable substrate, then carrying out the spin coating of an AgNWs dispersion liquid, and carrying out the annealing, so that an AgNWs thin film is formed on the stretchable substrate; the preparation method comprises the following steps: adding sulfimide salt into a PH 1000 solution, and stirring to obtain an S-PH 1000 solution; performing secondary oxygen plasma treatment on the AgNWs thin film, then spin-coating the AgNWs thin film with an S-PH1000 solution, and annealing to form an S-PH1000 film on the AgNWs thin film; and dropwise adding a sulfonyl imide salt aqueous solution into the S-PH1000 film, soaking, and annealing to obtain the stretchable substrate / AgNWs / S-PH1000 electrode, or stripping the stretchable substrate to obtain the AgNWs / S-PH1000 electrode. According to the preparation method, the composite electrode with high stretch rate, high light transmittance and high conductivity can be prepared. The invention also provides application of the stretchable transparent composite electrode prepared by the preparation method in flexible / stretchable electronic devices. The invention also provides a solar cell using the stretchable transparent composite electrode as an anode.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of composite materials, and specifically relates to a preparation method and application of a stretchable transparent composite electrode and a solar cell. Background Art

[0002] With the continuous advancement of technology, the application prospects of flexible electronic devices will be broader. In the future, we can foresee that electronic devices will be thinner, more flexible and wearable, which will not only be better integrated into our daily lives, but also bring revolutionary changes to medical health, energy management, information interaction and other fields. This will not only improve people's quality of life, but may also lead to new industrial changes and promote social progress. For wearable devices, in addition to meeting the functions of folding, bending and compression, they also need to be stretchable, so as to overcome the inevitable deformation of the device during use to meet the requirements of wearable power sources. Flexible batteries are the driving force for the work of flexible electronic products, and their development and utilization are directly related to the practical application of flexible electronics.

[0003] Among all current power technologies, Adv. Mater. 2023, 2307280; Energy Environ. Sci. 2023, 16, 2284 disclose that organic solar cells have the characteristics of ultra-flexibility, ultra-lightness, solution processing and translucency. Adv. Mater. 2024, 2400342; Natl. Sci. Rev. 2023, 10, nwad085 discloses that the best certified energy conversion efficiency of single-junction and stacked organic solar cells is as high as 19.79% and 20.3% respectively, making organic solar cells expected to play a unique role in wearable devices. Therefore, the development of intrinsically stretchable organic solar cells has become an essential element of wearable devices based on organic solar cells.

[0004] However, achieving both high performance and good stretchability is challenging, which requires the coordinated optimization of the substrate, transparent electrode, opaque electrode, active layer, and interface layer materials of organic solar cells to achieve good stretchability without sacrificing optoelectronic performance. Among the above factors, the development of stretchable transparent electrodes is the key to the development of intrinsically stretchable organic solar cells.

[0005] The document Nat.Electron.2019,2,513 discloses that silver nanowires (AgNWs) are widely used due to their excellent optoelectronic properties, superior flexibility and good solution processability. However, silver nanowires have two inherent disadvantages, namely high surface roughness and low adhesion, which may cause short circuits and reduced mechanical stability of silver nanowire electrodes. PH1000 has attracted widespread attention due to its excellent mechanical flexibility, adjustable work function and processability.

[0006] However, existing research has found it difficult to efficiently achieve a balance between the optical, electrical, and stretchability properties of PH1000 films.

[0007] Obviously, more reliable and superior stretchable electrode materials need to be developed to simultaneously achieve high performance and excellent mechanical properties of intrinsically stretchable organic solar cells. Summary of the invention

[0008] The invention provides a method for preparing a stretchable transparent composite electrode, which can prepare a composite electrode with high stretchability, high light transmittance and high conductivity.

[0009] The present invention provides a method for preparing a stretchable transparent composite electrode, comprising:

[0010] S1, subjecting the stretchable substrate to a first oxygen plasma treatment, and then subjecting the stretchable substrate to water vapor annealing to form a water vapor layer on the surface of the stretchable substrate, and then spin coating an AgNWs dispersion and annealing to obtain an AgNWs film;

[0011] Add the sulfonimide salt to the PH1000 solution and stir to obtain an S-PH1000 solution;

[0012] S2, subjecting the AgNWs film to a second oxygen plasma treatment, and then spin-coating the S-PH1000 solution on the AgNWs film, and annealing to obtain an S-PH1000 film;

[0013] S3, dropping a sulfonimide salt aqueous solution onto the S-PH1000 film, soaking for 0.5-10 min and then annealing to obtain a stretchable substrate / AgNWs / S-PH1000 electrode;

[0014] Alternatively, the stretchable substrate can be peeled off to obtain the AgNWs / S-PH1000 electrode.

[0015] The present invention spin-coats a silver nanowire (AgNWs) dispersion onto a water vapor layer, and the silver nanowires are dispersed in a solvent through small organic molecules in the dispersion. The water vapor layer improves the wettability of the silver nanowire solution on a substrate through a large surface tension difference between ethanol and water molecules, so that the AgNWs are uniformly dispersed and coated on a stretchable substrate without obvious aggregation and orientation, thereby increasing the light transmittance of the prepared electrode. Through annealing in step S1, the organic molecules on the surface of the AgNWs are removed, a high conductive network is achieved, and the current transmission performance is improved.

[0016] The present invention forms hydrophilic groups on the AgNWs film by performing a second oxygen plasma treatment on the AgNWs film, so that the AgNWs film and S-PH1000 form ohmic contact, which is beneficial to the transmission of electrons.

[0017] The present invention adds a BTSL aqueous solution to the S-PH1000 film of a stretchable substrate / AgNWs / S-PH1000 to dissolve and remove the insulating PSS of the S-PH1000, thereby improving the electron transport performance.

[0018] The PH1000 provided by the present invention is a specific model of the conductive polymer poly(3,4-ethylenedioxythiophene)-polystyrene sulfonic acid (PEDOT:PSS), which can be directly obtained through commercial channels.

[0019] Preferably, the power of the first oxygen plasma treatment is 100-800W, and the treatment time is 5-50s. Too high power or too long a time may cause damage to the substrate, such as material damage, too thick an oxide layer, or deformation of the substrate, thereby affecting the optical properties of the material. Preferably, the temperature of the water vapor annealing is room temperature, and the time is 1-5min.

[0020] Preferably, the concentration of the AgNWs dispersion is 1-5 mg / ml. If the concentration is too high, the AgNWs are likely to aggregate and form clusters during the film formation process, which increases the roughness of the AgNWs film and reduces the light transmittance.

[0021] Preferably, the annealing temperature in step S1 is 130-200° C. and the annealing time is 15-120 min.

[0022] The present invention controls the annealing temperature and time so that the organic molecules on the surface of the silver nanowires are removed, thereby improving the contact between the silver nanowires and reducing the square resistance, thereby improving the transmission efficiency of electrons. Excessively high temperature will cause deformation of the flexible substrate. The specific processing temperature is related to the selected substrate and cannot exceed the maximum temperature that the substrate can withstand.

[0023] Preferably, the sulfonyl imide salt is bis(trifluoromethane)sulfonyl imide lithium (BTSL), and in the raw material composition of the S-PH1000 membrane, based on the mass percentage of the solute in S-PH1000 being 100%, the mass percentage of BTSL accounts for 10 to 60 wt%.

[0024] The present invention controls the content of BTSL so that the formed S-PH1000 film has higher tensile properties and conductivity, further improving the conductivity at the place where the silver nanowires are not overlapped, thereby achieving high conductivity under high tensile conditions.

[0025] Preferably, the power of the second oxygen plasma is 100-800 W, and the duration is 5-50 s. By controlling the power and duration of the second oxygen plasma, the hydrophobic AgNWs film surface is made hydrophilic, which is beneficial to the coating of the S-PH1000 solution.

[0026] Preferably, the annealing temperature of step S2 is 100-150° C. and the time is 5-20 min. By controlling the annealing temperature and time, the crystallinity of the S-PH1000 film is better, which is beneficial to the transmission of electrons.

[0027] Preferably, the concentration of the sulfonimide salt aqueous solution in step S3 is 2-20 mg / ml, and the infiltration time is 0.5-10 min.

[0028] Preferably, the stretchable substrate is at least one of polyurethane (TPU), polydimethylsiloxane (PDMS), styrene-ethylene-butylene-styrene block copolymer (SEBS), and styrene-ethylene / propylene-styrene block copolymer (SEPS).

[0029] Preferably, the thickness of the stretchable substrate of the stretchable transparent composite electrode is 10 to 300 μm, the thickness of the AgNWs film is 30 to 50 nm, and the thickness of the S-PH1000 film is 50 to 110 nm.

[0030] On the other hand, the present invention also provides a stretchable transparent composite electrode, which is prepared by the preparation method of the stretchable transparent composite electrode.

[0031] On the other hand, the present invention also provides the use of the stretchable transparent composite electrode in flexible / stretchable electronic devices, which include display screens, solar cells, smart sensors, electronic skin, supercapacitors or batteries.

[0032] On the other hand, the present invention further provides a solar cell, comprising, from bottom to top:

[0033] substrate;

[0034] an anode, wherein the anode is the stretchable transparent composite electrode;

[0035] A hole transport layer, the hole transport layer being located on the S-PH1000 film of the stretchable transparent composite electrode;

[0036] Active layer;

[0037] Electron transport layer;

[0038] and cathode.

[0039] The present invention uses the stretchable transparent composite electrode as an anode and utilizes the uniformly dispersed distribution of silver nanowires to avoid the increase of local roughness due to obvious aggregation and orientation of the silver nanowires, thereby avoiding piercing the solar cell.

[0040] Preferably, the substrate is glass, silicon or a stretchable substrate, and the stretchable substrate is at least one of polyurethane (TPU), polydimethylsiloxane (PDMS), styrene-ethylene-butylene-styrene block copolymer (SEBS), and styrene-ethylene / propylene-styrene block copolymer (SEPS).

[0041] Preferably, the solar cell further comprises an anode modification layer, wherein the anode modification layer is located between the anode and the hole transport layer, and the anode modification layer is a PCP-2F-Li thin film.

[0042] The present invention uses the PCP-2F-Li film as an anode modification layer to compensate for the problem of insufficient hydrophilicity of the S-PH1000 film due to the dissolution of the hydrophilic PSS, so that the physical contact of the S-PH1000 film is better, so that it can be better combined with the hole transport layer. The present invention can also improve the work function of the stretchable transparent composite electrode by adding PCP-2F-Li, so that the energy level difference after the combination with the hole transport layer is small, the attenuation during the electron transmission process is small, which is beneficial to the effective charge collection of the organic solar cell.

[0043] Preferably, the preparation method of the PCP-2F-Li film is: coating a methanol solution of PCP-2F-Li on an S-PH1000 film of a stretchable transparent composite electrode to obtain a PCP-2F-Li / stretchable transparent composite electrode.

[0044] The PCP-2F-Li is a 3 to 15 nm thick polylithium 3,3'-(2-(2,2'-difluoro-4'-methyl-[1,1'-biphenyl]-4-yl)-6-methyl-4H-cyclopentyl[2,1-b:3,4-b']dithiophene-4,4-diyl)bis(propane-1-sulfonate).

[0045] More preferably, the concentration of the PCP-2F-Li methanol solution is 0.5-2 mg / ml.

[0046] Preferably, the hole transport layer is PEDOT:PSS (model AI4083);

[0047] The electron transport layer is zinc oxide nanoparticles;

[0048] The cathode is an EGaIn electrode;

[0049] The active layer is a multi-component blended membrane, and its raw material composition includes a polymer donor PM6, an L8-BO acceptor and a styrene-ethylene / propylene-styrene block copolymer (SEPS).

[0050] Without adding SEPS, the active layer still has stretchable properties. When SEPS is added, the stretching ability of the active layer increases with the increase of SEPS, and the photovoltaic performance of the device decreases with the increase of SEPS. When the addition amount is 10%, the tensile performance and photovoltaic performance of the device reach a good balance. The specific implementation can adjust the amount of SEPS added as needed. The amount of SEPS added provided by the present invention is 2-20%. For example, preferably, based on the total mass of the polymer donor PM6 and the L8-BO acceptor as 100%, the amount of SEPS added can be 10%.

[0051] The molecular structures of PM6 and L8-BO are shown below:

[0052]

[0053] The anode provided by the present invention is a stretchable transparent composite electrode. In addition to having high electrical conductivity and stretchability, the high light transmittance of the composite electrode can further improve the light absorption rate of the active layer, thereby improving the photoelectric energy conversion efficiency of the organic solar cell.

[0054] Preferably, the hole transport layer is PEDOT:PSS, and the thickness of the hole transport layer is 10 to 30 nm;

[0055] The thickness of the active layer is 50 to 300 nm;

[0056] The thickness of the electron transport layer is 10 to 30 nm;

[0057] The thickness of the cathode is 30-300 nm.

[0058] The specific model of the PEDOT:PSS may be AI4083, which can be directly obtained through commercial channels.

[0059] Compared with the prior art, the present invention has the following beneficial effects:

[0060] The present invention spin-coats an AgNWs dispersion on a water vapor layer, so that fine AgNWs are evenly dispersed on a stretchable substrate, thereby increasing light transmittance. The organic molecules on the surface of the AgNWs are removed by annealing to reduce square resistance. During the stretching process, the conductivity of S-PH1000 can be used to transmit current at un-overlapped portions. At the same time, since both AgNWs and S-PH1000 have good stretching properties, the electrode prepared by the present invention still has high conductivity at a high stretching rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0061] Figure 1 The tensile strain-conductivity curve of the S-PH1000 transparent electrode prepared in Comparative Example 1;

[0062] Figure 2 The transmittance curves of the composite electrodes prepared from the AgNW dispersions of different concentrations obtained in Example 1;

[0063] Figure 3 The square resistance curves of the AgNWs / S-PH1000 composite transparent electrodes with different concentrations prepared in Example 1;

[0064] Figure 4 The tensile strain-conductivity curve of the AgNWs / S-PH1000 composite transparent electrode prepared in Example 1;

[0065] Figure 5 The current-voltage curves of the solar cells prepared in Comparative Example 2, Example 2 and Example 4;

[0066] Figure 6 Ultraviolet photoelectron spectroscopy (UPS) diagrams of S-PH1000 prepared in Comparative Example 3, and AgNWs / S-PH1000 and AgNWs / S-PH1000 / PCP-2F-Li thin films prepared in Example 3;

[0067] Figure 7 This is a contact angle effect diagram of the glass / AgNWs / S-PH1000 / PCP-2F-Li electrode prepared in Example 3;

[0068] Figure 8 The current-voltage curves of the solar cell (0% SEPS) prepared in Example 5 and the solar cell (10% SEPS) prepared in Example 6;

[0069] Fig. 9 This is a graph showing the energy conversion efficiency retention rate of the solar cell prepared in Example 6 at different strains;

[0070] Fig.10 This is a curve of the stretching times-energy conversion efficiency retention rate of the solar cell prepared in Example 6 at a tensile strength of 20%. DETAILED DESCRIPTION

[0071] The present invention will be further described below in conjunction with the accompanying drawings and specific embodiments. It should be understood that these embodiments are only used to illustrate the present invention and are not used to limit the scope of the present invention.

[0072] In the following embodiments, different types of anodes have slightly different preparation processes, so the thickness of different types of anodes under optimal conditions is slightly different. The thickness of the anode in the following embodiments is the optimal thickness matching the anode type.

[0073] The transmittance detection method used in the embodiments provided by the present invention is UV-visible absorption spectroscopy, and the background subtraction of the substrate transmittance is performed during the test process. For example, the transmittance obtained in Example 1 is the transmittance data of the composite electrode AgNWs / S-PH1000.

[0074] The conductivity detection method used in the embodiment provided by the present invention is divided into using a four-probe tester to test the square resistance of the film, and then using the formula conductivity = 1 / (square resistance*film thickness) to calculate the conductivity of the film.

[0075] Comparative Example 1

[0076] This comparative example provides a method for preparing a TPU / S-PH1000 electrode, and the specific steps are as follows:

[0077] S1. Spin-coat a DMF solution (200 mg / ml) of polyurethane (TPU) on a 1.5 cm × 1.5 cm glass sheet at 800 rpm for 1 min and dry at 80 °C for 5 h. The prepared TPU film (50 μm) was treated under 150 W oxygen plasma for 30 s to improve wettability.

[0078] S2, 40wt% BTSL was added to PH1000, stirred vigorously for 15min, and S-PH1000 was spin-coated on the surface of TPU treated with oxygen plasma at room temperature, and annealed at 130℃ for 10min. Then, 10mg / ml BTSL aqueous solution was dropped on the S-PH1000 film for post-treatment, waited for 1min, spun at 4000rpm for 20S to remove the liquid, and then annealed at 130℃ for 10min.

[0079] S3. Then, the polyurethane is peeled off from the glass substrate to obtain the TPU / S-PH1000 electrode.

[0080] The TPU / S-PH1000 electrodes prepared in this comparative example are fixed at both ends of the tensile test instrument with a spacing of 1 cm. Figure 1 , when stretched, the conductivity along the stretching direction (||) increases to nearly 1.5 times the initial value, and then continues to decline. However, the conductivity continues to decrease in the perpendicular direction (⊥). At 0-50% strain, the conductivity remains above 1000S / cm, reaches a maximum of 1587S / cm at 30% strain, and reaches a maximum of more than 100S / cm at 200% strain.

[0081] Example 1

[0082] This embodiment provides a method for preparing a TPU / AgNWs / S-PH1000 electrode, and the specific steps are as follows:

[0083] S1. Spin-coat a DMF solution (200 mg / ml) of polyurethane (TPU) on a 1.5 cm×1.5 cm glass sheet at 800 rpm for 1 minute and dry at 80°C for 5 hours to obtain a TPU film (50 μm). Treat the film under 150 W oxygen plasma for 30 seconds to improve wettability, and anneal with water vapor to form a water vapor layer on the surface of the TPU substrate. Dilute an AgNWs dispersion (the silver nanowire dispersion is provided by Zhejiang Kechuang Advanced Materials Co., Ltd., and the size of the silver nanowires is 25-30 nm in diameter and 10-30 μm in length) to 5, 4, 3, 2, and mg / ml, then spin-coat the AgNWs dispersion of this concentration on the TPU with a water vapor layer on the surface, and anneal at 150°C for 20 minutes to form an AgNWs film on the TPU.

[0084] 40 wt % of BTSL was added to PH1000 and stirred vigorously for 15 min to obtain S-PH1000 solution.

[0085] S2. Spin-coat the S-PH1000 solution on the surface of the AgNWs film at room temperature and anneal at 130°C for 10 min to obtain the S-PH1000 film.

[0086] S3, then drop 10 mg / ml BTSL aqueous solution on the S-PH1000 film for post-treatment, wait for 1 min, rotate at 4000 rpm for 20 s to remove the liquid, and then anneal at 130 °C for 10 min. Then, the polyurethane was torn off the glass substrate to obtain the TPU / AgNWs / S-PH1000 electrode.

[0087] like Figure 2 As shown, the transmittance of the composite electrodes prepared with 5, 4, 3 and 2 mg / ml AgNW dispersions at 550 nm is 93.4%, 93.7%, 94.4% and 94.9%, respectively. It can be seen that the prepared composite electrodes have excellent optical properties.

[0088] The square resistance of the composite electrode prepared in the test example is as follows: Figure 3 As shown, the quality factor (FoM) of the composite electrode is calculated using the formula:

[0089]

[0090] Among them, σ dc is the DC conductivity, σ op is the photoconductivity, R shis the sheet resistance, T is the transmittance, and λ is 550nm. The quality factors of the composite electrodes prepared with 5, 4, 3, and 2 mg / ml AgNW dispersions are 246.7, 190.0, 161.2, and 122.6, respectively. It can be seen that the electrode prepared with 5 mg / ml AgNW dispersion has the highest quality factor.

[0091] The TPU / AgNWs / S-PH1000 electrodes prepared in this example were fixed at both ends of the tensile test instrument with a spacing of 1 cm. Figure 4 ,When stretched, the TPU / AgNWs / S-PH1000 film made of 5mg / ml AgNWs dispersion continued to decrease along the stretching direction (||) and the vertical direction (⊥), and the conductivity in the stretching direction decreased faster than that in the vertical direction. It can be seen that the TPU / AgNWs / S-PH1000 composite electrode can still maintain good conductivity under 60% strain.

[0092] Comparative Example 2

[0093] This comparative example provides a method for preparing a solar cell, and the specific steps are as follows:

[0094] The glass substrate was treated with an ultraviolet ozone generator for 15 minutes.

[0095] 40 wt % BTSL was added to PH1000 and stirred vigorously for 15 min to obtain S-PH1000. S-PH1000 was spin-coated on a glass surface treated with oxygen plasma at room temperature and annealed at 130 ° C for 10 min to obtain an S-PH1000 film. Then, 10 mg / ml BTSL aqueous solution was dropped on the S-PH1000 film for post-treatment. After waiting for 1 min, the film was rotated at 4000 rpm for 20 s to remove the liquid and annealed at 130 ° C for 10 min to obtain the anode.

[0096] Then, the PSS-removed S-PH1000 film of the anode electrode was patterned under a 532 nm nanosecond laser beam, and then a 20 nm thick PEDOT:PSS (model AI4083) film was spin-deposited as a hole transport layer;

[0097] Then, the substrate was baked in air at 150°C for 15 min and transferred to a glove box. PM6:L8-BO (weight ratio of 1:1.2) was spun at 2600 rpm for 20 s in a 16.5 mg / mL chloroform:DIO (volume ratio of 99.75:0.25) solution and annealed at 80°C for 5 min to obtain an active layer with a thickness of about 80 nm.

[0098] Then, a 5 nm thick PDINN film was spin-coated with a 1 mg / ml methanol solution as an electron transport layer.

[0099] Then, a 100 nm thick Ag film was deposited by thermal evaporation as the cathode with an active area of ​​6 mm 2 , the test aperture area is 4.78mm 2 .

[0100] At a light intensity of 100 mW / cm 2 The current-voltage curve of the solar cell prepared in this comparative example is tested under the AM1.5 simulated sunlight. Figure 5 The corresponding curve of S-PH1000 shows that the open circuit voltage is 0.876 V and the short circuit current density is 23.75 mA / cm 2 , the filling factor is 68.81% and the energy conversion efficiency is 14.31%.

[0101] Example 2

[0102] This embodiment provides a method for preparing a solar cell, and the specific steps are as follows:

[0103] The glass substrate was treated with an ultraviolet ozone generator for 15 minutes, and annealed with water vapor to form a water vapor layer on the surface of the glass substrate treated with oxygen plasma.

[0104] The AgNWs dispersion was diluted to 5 mg / ml, and the 5 mg / ml AgNWs dispersion was spin-coated on the TPU with a water vapor layer formed on the surface, and annealed at 150° C. for 20 min to obtain an AgNWs film.

[0105] 40wt% BTSL was added to PH1000 and stirred vigorously for 15min to obtain S-PH1000. S-PH1000 was spin-coated on the surface of the AgNWs film at room temperature and annealed at 130°C for 10min to obtain the S-PH1000 film. Then, 10mg / ml BTSL aqueous solution was dropped on the S-PH1000 film for post-treatment. The film was waited for 1min and rotated at 4000rpm for 20s to remove the liquid. The film was annealed at 130°C for 10min to obtain the S-PH1000 film with PSS removed, thereby obtaining glass substrate / AgNWs / S-PH1000.

[0106] The S-PH1000 film with PSS removed was then patterned under a 532 nm nanosecond laser beam, and then a 20 nm thick PEDOT:PSS (model AI4083) film was spin-deposited as a hole transport layer.

[0107] Then it was baked in air at 150°C for 15 min, and the substrate was transferred to a glove box. PM6:L8-BO (weight ratio of 1:1.2) was rotated at 2600 rpm for 20 s in a 16.5 mg / mL chloroform:DIO (volume ratio of 99.75:0.25) solution and annealed at 80°C for 5 min to obtain an active layer with a thickness of about 80 nm.

[0108] Then, a 5 nm thick PDINN film was spin-coated with a 1 mg / ml methanol solution as an electron transport layer.

[0109] Then, a 100 nm thick Ag film was deposited by thermal evaporation as the cathode with an active area of ​​6 mm 2 , the test aperture area is 4.78mm 2 .

[0110] At a light intensity of 100 mW / cm 2 The current-voltage curve of the solar cell prepared in this embodiment is tested under the AM1.5 simulated sunlight. Figure 5 The corresponding curve of AgNWs / S-PH1000 is shown in Figure 2, from which the open circuit voltage is 0.874 V and the short circuit current density is 25.08 mA / cm 2 , the filling factor is 77.18% and the energy conversion efficiency is 16.95%.

[0111] Comparative Example 3

[0112] This comparative example provides a method for preparing a Si / S-PH1000 electrode, and the specific steps are as follows:

[0113] Treat the silicon (Si) substrate with an ultraviolet ozone generator for 15 minutes. Then add 10-60wt% BTSL to PH1000, stir vigorously for 15 minutes, spin-coat S-PH1000 on the Si surface at room temperature, and anneal at 130°C for 10 minutes. Then drop 10mg / ml BTSL aqueous solution on the S-PH1000 film for post-treatment, wait for 1 minute, spin at 4000rpm for 20 seconds to remove the liquid, and then anneal at 130°C for 10 minutes. Obtain Si / S-PH1000 sample.

[0114] Example 3

[0115] This embodiment provides a method for preparing a Si / AgNWs / S-PH1000 / PCP-2F-Li electrode, and the specific steps are as follows:

[0116] The Si substrate was treated with an ultraviolet ozone generator for 15 minutes. The AgNWs dispersion was diluted to 5 mg / ml and annealed with water vapor to form a water vapor layer on the surface of the Si substrate. Then, the AgNWs dispersion of this concentration was spin-coated on the Si surface with the water vapor layer formed on the surface, and annealed at 150°C for 20 minutes to obtain the AgNWs film.

[0117] 40wt% BTSL was added to PH1000, and the mixture was stirred vigorously for 15min to obtain S-PH1000. S-PH1000 was spin-coated on the surface of AgNWs film at room temperature, and annealed at 130℃ for 10min to obtain S-PH1000 film. Then, 10mg / ml BTSL aqueous solution was dropped on the S-PH1000 film for post-treatment, and the film was waited for 1min, rotated at 4000rpm for 20s to remove the liquid, and then annealed at 130℃ for 10min. Si / AgNWs / S-PH1000 sample was obtained.

[0118] A methanol solution of PCP-2F-Li (1 mg / ml) was coated on the surface of the Si / AgNWs / S-PH1000 sample to obtain a Si / AgNWs / S-PH1000 / PCP-2F-Li sample.

[0119] Ultraviolet photoelectron spectroscopy (UPS) tested the work functions of S-PH1000 prepared in comparative example 3, and AgNWs / S-PH1000 and AgNWs / S-PH1000 / PCP-2F-Li films prepared in Example 3, which were 4.60, 4.48 and 4.84 eV, respectively. The poor matching between the electrode work function and the energy level of the hole transport layer may lead to charge accumulation or recombination at the interface, reduce the charge collection efficiency, and further affect the short-circuit current and fill factor of the battery. PCP-2F-Li modification increased the work function of AgNWs / S-PH1000 from 4.48 eV to 4.84 eV, which is closer to 5.10 eV of the hole transport layer AI4083, see Figure 6 .

[0120] The contact angle test showed that the contact angles of the AI4083 solution on the AgNWs / S-PH1000 and AgNWs / S-PH1000 / PCP-2F-Li thin films prepared in Example 3 were 98.3 and 41.3°, respectively. Figure 7 The reduced contact angle can enhance the physical contact between the composite electrode and the hole transport layer AI4083.

[0121] Example 4

[0122] A solar cell was prepared in this example. The preparation method was different from that in Example 2 in that the surface of the AgNWs / S-PH1000 / PCP-2F-Li composite electrode was modified with a 1 mg / ml PCP-2F-Li methanol solution before spin coating the hole transport layer.

[0123] Solar cells under a light intensity of 100mW / cm 2 The current-voltage curve of the solar cell prepared in this embodiment under the AM1.5 simulated sunlight is shown in FIG. Figure 5 The corresponding curve of AgNWs / S-PH1000 / PCP-2F-Li shows that the modification of PCP-2F-Li significantly improves the device efficiency from 16.95% to 17.34%, with an open circuit voltage of 0.879 V and a short circuit current of 25.15 mA cm -2 , the filling factor is 78.38%.

[0124] Example 5

[0125] This embodiment provides a method for preparing a solar cell, and the specific preparation steps are as follows:

[0126] The DMF solution (200 mg / ml) of polyurethane (TPU) was spin-coated on a 1.5 cm×1.5 cm glass sheet at 800 rpm for 1 min and dried at 80°C for 5 h. The prepared TPU film (50 μm) was treated under 150 W oxygen plasma for 30 s to improve wettability and annealed with water vapor to form a water vapor layer on the surface of the TPU substrate.

[0127] The AgNWs dispersion was diluted to 5 mg / ml, and then the AgNWs dispersion of this concentration was spin-coated on TPU with a water vapor layer on the surface, and annealed at 150° C. for 20 min to obtain an AgNWs film.

[0128] Then, 40 wt% BTSL solution was added to PH1000, and the mixture was stirred vigorously for 15 min to obtain S-PH1000, which was then spin-coated on the AgNWs film at room temperature and annealed at 130 °C for 10 min to obtain the S-PH1000 film. Then, 10 mg / ml BTSL aqueous solution was dropped on the S-PH1000 film for post-treatment, and the film was waited for 1 min, and then rotated at 4000 rpm for 20 s to remove the liquid, and then annealed at 130 °C for 10 min to obtain the S-PH1000 film with PSS removed.

[0129] Then, the hybrid electrode was patterned under a 532 nm nanosecond laser beam. Then, the surface of the AgNWs / S-PH1000 composite electrode was modified with a 1 mg / ml methanol solution of PCP-2F-Li.

[0130] Then, a 20 nm thick PEDOT:PSS (model AI4083) film was spin-deposited as a hole transport layer.

[0131] Then it was baked in air at 150°C for 15 min, the substrate was transferred to a glove box, PM6:L8-BO (weight ratio of 1:1.2) was spin-coated at 2600 rpm for 20 s in 16.5 mg / mL chloroform:DIO (volume ratio of 99.75:0.25) solution, and annealed at 80°C for 5 min to obtain an active layer with a thickness of about 80 nm.

[0132] Then, a 20 nm thick ZnO NPs cathode modification layer was spin-coated on the active layer using 8 mg / mL zinc oxide nanoparticle (ZnO NPs) methanol solution at a rotation speed of 3500 rpm.

[0133] Finally the top EGaIn electrode is deposited.

[0134] At a light intensity of 100 mW / cm 2 The current-voltage curve of the solar cell prepared in this embodiment was tested under AM1.5 simulated sunlight, from which the open circuit voltage was found to be 0.871 V and the short circuit current density was 25.44 mA / cm 2 , the filling factor is 73.66%, the PCE is 16.32%, see Figure 8 .

[0135] Example 6

[0136] The difference from Example 5 is that 10% by mass (based on the total mass of PM6 and L8-BO as 100%) of SEPS is added to the chloroform mixed solution used to make the active layer, and a device having SEPS in the active layer is obtained. Figure 8 It is recorded as 10% SEPS.

[0137] See also Figure 8 , at a light intensity of 100mW / cm 2 The current-voltage curve of the 10% SEPS device was tested under AM1.5 simulated sunlight, from which the open circuit voltage was 0.872V and the short circuit current density was 24.22mA / cm 2 , the filling factor is 72.02% and the PCE is 15.20%.

[0138] from Fig. 9 It can be seen that the introduction of SEPS in the active layer can improve the stretchability of the device.

[0139] from Fig.10It can be seen that the device with 10% SEPS in the active layer has excellent performance based on the AgNWs / S-PH1000 composite electrode.

[0140] The AgNWs / PH1000 composite electrode prepared in this embodiment achieved a quality factor of 246.7, which is the highest value of stretchable transparent electrodes at present. At the same time, the composite electrode also has excellent stretchability and can still maintain good conductivity under 60% strain. The energy conversion efficiency of the intrinsically stretchable organic solar cell based on the AgNWs / PH1000 composite electrode prepared in this embodiment can reach 16.32%, which is the highest value of intrinsically stretchable organic solar cells at present.

[0141] The transparent electrode used in the present invention is a composite stretchable electrode of silver nanowires / conductive polymer (named AgNWs / S-PH1000) formed by introducing a layer of conductive polymer layer S-PH1000 with stretchability on the silver nanowire electrode. In the composite electrode, the deposition of silver nanowires greatly improves the conductivity of the composite electrode, and the uniformly diluted and dispersed silver nanowires improve the light transmission efficiency of the electrode, which is beneficial to the improvement of device performance. The conductive polymer provides good stretchability and can form a continuous conductive network during the stretching process. At the same time, the coating of the conductive polymer greatly reduces the roughness of the silver nanowire film, making AgNWs / S-PH1000 more suitable for use as a transparent bottom electrode. This composite electrode strategy simultaneously maximizes the optical, electrical and mechanical properties of the electrode.

[0142] The silver nanowires used in the present invention are prepared by annealing the substrate solvent (water) vapor, and then coating the diluted silver nanowire dispersion on the substrate using a spin coating process. The water vapor treatment improves the wettability of the silver nanowire solution on the substrate through the large surface tension difference between ethanol and water molecules, thereby obtaining a uniformly dispersed silver nanowire film, thereby improving the optical and electrical properties of the silver nanowire film. Diluting the silver nanowire dispersion can further improve the optical properties of the silver nanowire film, so that the silver nanowires can further improve the transmittance of the silver nanowire film while maintaining a high conductive network.

[0143] The S-PH1000 film used in the present invention is prepared by introducing lithium bis(trifluoromethane)sulfonyl imide to improve the stretchability and conductivity of the S-PH1000 film, and eluting the S-PH1000 with a lithium bis(trifluoromethane)sulfonyl imide solution to remove part of the PSS in the film, thereby further improving the conductivity.

[0144] The PCP-2F-Li buffer layer used in the present invention can modify the surface of the AgNWs / S-H1000 electrode, thereby improving the electrode work function and the physical contact between the electrode and the interface layer. The modification of the PCP-2F-Li buffer layer is beneficial to the effective charge collection of the organic solar cell, thus realizing a high-performance intrinsically stretchable organic solar cell.

[0145] In addition, it should be understood that after reading the above description of the present invention, those skilled in the art may make various changes or modifications to the present invention, and these equivalent forms also fall within the scope defined by the claims attached to this application.

Claims

1. A method for preparing a stretchable transparent composite electrode, characterized in that: include: S1, performing a first oxygen plasma treatment on the stretchable substrate, then performing water vapor annealing to form a water vapor layer on the surface of the stretchable substrate, spin coating an AgNWs dispersion, and annealing to obtain an AgNWs film; Add the sulfonimide salt to the PH1000 solution and stir to obtain an S-PH1000 solution; S2, subjecting the AgNWs film to a second oxygen plasma treatment, and then spin-coating the S-PH1000 solution on the AgNWs film, and annealing to obtain an S-PH1000 film; S3, dropping a sulfonimide salt aqueous solution onto the S-PH1000 film, soaking for 0.5-10 min and then annealing to obtain a stretchable substrate / AgNWs / S-PH1000 electrode; Alternatively, the stretchable substrate can be peeled off to obtain the AgNWs / S-PH1000 electrode.

2. The method for preparing a stretchable transparent composite electrode according to claim 1, characterized in that: The power of the first oxygen plasma treatment is 100-800W, and the treatment time is 5-50s.

3. The method for preparing a stretchable transparent composite electrode according to claim 1, characterized in that: The concentration of the AgNWs dispersion is 1-5 mg / ml.

4. The method for preparing a stretchable transparent composite electrode according to claim 1, characterized in that: The annealing temperature in step S1 is 130-200° C. and the annealing time is 15-120 min.

5. The method for preparing a stretchable transparent composite electrode according to claim 1, characterized in that: The sulfonyl imide salt is lithium bis(trifluoromethane)sulfonyl imide (BTSL). In the raw material composition of the S-PH1000 membrane, based on the mass percentage of the solute in S-PH1000 being 100%, the mass percentage of lithium bis(trifluoromethane)sulfonyl imide accounts for 10 to 60 wt%.

6. The method for preparing a stretchable transparent composite electrode according to claim 1, characterized in that: In step S3, the stretchable substrate is at least one of polyurethane, polydimethylsiloxane, styrene-ethylene-butylene-styrene block copolymer, and styrene-ethylene / propylene-styrene block copolymer.

7. Application of a stretchable transparent composite electrode prepared by the method for preparing a stretchable transparent composite electrode as claimed in any one of claims 1 to 6 in a flexible / stretchable electronic device.

8. A solar cell, characterized in that: From bottom to top they include: substrate; an anode, wherein the anode is a stretchable transparent composite electrode prepared by the method for preparing a stretchable transparent composite electrode according to any one of claims 1 to 6; A hole transport layer, the hole transport layer being located on the S-PH1000 film of the stretchable transparent composite electrode; Active layer; Electron transport layer; and cathode.

9. The solar cell according to claim 8, characterized in that The solar cell further comprises an anode modification layer; The anode modification layer is located between the anode and the hole transport layer, and the anode modification layer is a PCP-2F-Li film.

10. The solar cell according to claim 8, characterized in that The hole transport layer is PEDOT:PSS; The electron transport layer is zinc oxide nanoparticles; The cathode is an EGaIn electrode; The active layer is a multi-component blended membrane, and its raw material composition includes a polymer donor PM6, an L8-BO acceptor and a styrene-ethylene / propylene-styrene block copolymer.