Method for evaluating surface defects of bar steel

Through flaw detection data analysis and the use of defect density index, the characteristics of rod steel surface defects are automatically evaluated, which solves the problem of lack of defect trait evaluation in the prior art, and improves the pertinence and yield of manufacturing conditions.

CN118984934APending Publication Date: 2024-11-19JFE STEEL CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202280094363.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Priority Date
2022-03-30
Filing Date
2022-12-08
Publication Date
2024-11-19

AI Technical Summary

Technical Problem

The prior art lacks evaluation of defect characteristics in the detection of surface defects of rod steel, which leads to insufficient countermeasures to inhibit defect generation and affect the yield rate.

Method used

Through flaw detection data analysis, the correlation between the characteristics of the surface defect of the rod steel and the data pattern was found in advance, and the characteristics of the surface defect of the rod steel are automatically evaluated using the defect density index to determine the optimal manufacturing conditions.

Benefits of technology

The accuracy of trait recognition of rod steel defects has been improved, the determination of defect suppression measures has been simplified, and the yield rate has been improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118984934A_ABST
    Figure CN118984934A_ABST
Patent Text Reader

Abstract

The purpose of the present invention is to make it possible to evaluate the properties of defects occurring in a steel bar on the basis of a plurality of pieces of flaw detection data obtained by flaw detection of the surface of the steel bar. And a surface defect evaluation method for evaluating the properties of the surface defects of the bar steel. The correlation between the characteristics of the surface defects of the steel bar and the characteristics of a data pattern obtained by flaw detection along the surface of the steel bar is determined in advance. On the basis of the correlation and the characteristics of a data pattern obtained by performing flaw detection on the bar steel (1) to be evaluated, the properties of the surface defects of the bar steel (1) to be evaluated, which is the bar steel for which the properties of the surface defects have been evaluated, are identified.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technique for evaluating the properties of surface defects generated in a steel bar. Background Art

[0002] Conventionally, surface defects of steel bar products are inspected by moving a magnetic flux leakage detector, eddy current detector, or other flaw detector along the surface of the steel bar to inspect the entire surface, as described in Patent Document 1. In addition, defects above a predetermined level are considered as defects to be detected, and whether or not there are defects above the predetermined level in the product is evaluated.

[0003] In this case, as in Patent Document 2, there is also a technology for detecting minute defects with high accuracy.

[0004] In addition, when the entire circumference of the steel bar is to be inspected, the flaw detector is relatively moved in the circumferential direction of the steel bar and also in the longitudinal direction as in Patent Document 3. Thus, the entire circumference of the surface of the steel bar is scanned to determine whether or not there are defects exceeding a predetermined value on the surface of the steel bar.

[0005] Prior art literature

[0006] Patent Literature

[0007] Patent Document 1: Japanese Patent Application Publication No. 2001-41932

[0008] Patent Document 2: Japanese Patent Application Publication No. 2009-68857

[0009] Patent Document 3: Japanese Patent Application Publication No. 2017-167057 Summary of the invention

[0010] Problems to be solved by the invention

[0011] Conventional flaw detection methods for steel bars are intended to detect with high accuracy whether or not there are defects on the surface of the steel bar that are larger than a predetermined level, rather than to evaluate the properties (state) of the surface defects.

[0012] However, in future steel bar production, measures for suppressing defects on the steel bar surface may differ depending on the properties of the defects that occur.

[0013] In the study of improvement measures, unlike the detection of the presence or absence of defects above the prescribed level as described above, the operator actually confirms the state (properties) of the defects on the surface of the defective steel bar by visual inspection. Then, based on the state of the confirmed defects, measures to suppress the occurrence of the defects in future steel bar manufacturing are determined.

[0014] As described above, conventional flaw detection methods aim to detect flaws without omission in order to determine whether the current steel bar is acceptable as a product. However, conventional flaw detection methods do not evaluate the properties of the flaws for countermeasures on the production line.

[0015] The present invention has been made in view of the above problems, and its object is to enable the properties of defects generated in a steel bar to be evaluated based on a plurality of flaw detection data obtained by flaw detection on the surface of the steel bar. In other words, the present invention aims to provide a technology that can automatically distinguish the properties of defects based on the flaw detection data.

[0016] Means for solving problems

[0017] In order to solve the problem, one embodiment of the present invention is directed to a surface defect evaluation method for evaluating properties of surface defects of a steel bar, wherein a correlation between properties of surface defects of the steel bar and features of a data pattern obtained by flaw detection along the surface of the steel bar is obtained in advance, and the properties of surface defects of the steel bar to be evaluated are determined based on the correlation and the features of the data pattern obtained by flaw detection on the steel bar to be evaluated, wherein the steel bar to be evaluated is a steel bar for which properties of surface defects are evaluated.

[0018] Effects of the Invention

[0019] Depending on the properties (state) of defects generated on the surface, the direction of optimization of the operating conditions for producing steel bars to reduce the defects varies.

[0020] In contrast, according to the present invention, the properties of the surface defects actually generated are not evaluated by visual inspection, but the properties of the defects are evaluated based on the flaw detection data. Therefore, according to the present invention, it is easy to identify (evaluate) which defects have occurred in which steel bar product.

[0021] As a result, according to the aspect of the present invention, it is easy to confirm the optimal manufacturing conditions for each product for defect suppression measures, thereby improving the yield. BRIEF DESCRIPTION OF THE DRAWINGS

[0022] [ Figure 1 ] is a conceptual diagram showing an example of a device for defect evaluation based on an embodiment of the present invention.

[0023] [ Figure 2 ] is a diagram illustrating two examples of flaw detection images and an example of detecting the presence or absence of defects based on the flaw detection images.

[0024] [ Figure 3 ] is a diagram showing the relationship between the first partition D1 and the second partition D2.

[0025] [ Figure 4] is an indexed diagram illustrating the characteristics of the flaw detection image (data pattern).

[0026] [ Figure 5 ] are figures showing examples of the properties of defects, (a) is a length direction defect 1, (b) is a length direction defect 2, and (c) is an example of a single flaw.

[0027] [ Figure 6 ] are diagrams showing examples of the properties (features) of the flaw detection diagram (data pattern) under the properties of each defect and a diagram of the defect density index at that time. (a) is an example of the case of a longitudinal defect 1, (b) is an example of the case of a longitudinal defect 2, and (c) is an example of the case of a single defect.

[0028] [ Figure 7 ] are diagrams showing the characteristics of the properties of each defect in the flaw detection diagram. (a) is an example of the case of a lengthwise defect 1, (b) is an example of the case of a lengthwise defect 2, and (c) is an example of the case of a single defect. DETAILED DESCRIPTION

[0029] Hereinafter, embodiments according to the present invention will be described with reference to the drawings.

[0030] (constitute)

[0031] Steel bars are manufactured, for example, in a steel bar factory equipped with a heating furnace, a roughing mill, an intermediate mill, and a finishing mill. The manufactured steel bars are evaluated for surface quality using, for example, a magnetic flux leakage flaw detector in a finishing factory.

[0032] like Figure 1 As shown, the flaw detection equipment of this embodiment includes a flaw detection device and a flaw detection control unit 3.

[0033] <Flaw detection device>

[0034] like Figure 1 As shown, the flaw detector 2 is close to the surface of the steel bar 1 to scan the surface of the steel bar 1 in the circumferential direction and the longitudinal direction (axial direction). Then, the flaw detector continuously detects flaws on the entire surface of the steel bar 1 based on the scanned information.

[0035] As the flaw detector 2 and the flaw detection method using the flaw detector 2, the configuration of the flaw detector 2 and the flaw detection method known in the past may be adopted. The configuration of the flaw detector 2 and the flaw detection method are not particularly limited.

[0036] The flaw detection device of the present embodiment includes a flaw detector 2 such as a magnetic flux leakage flaw detector or an eddy current flaw detector. Then, the flaw detector 2 performs flaw detection on the entire surface of the steel bar 1 to be inspected.

[0037] <Flaw Detection Control Department 3>

[0038] like Figure 1 As shown, the flaw detection control unit 3 includes a flaw detection data generating unit 3A, a defect determination unit 3B, and a defect property evaluation unit 3C.

[0039] <Flaw Detection Data Generator 3A>

[0040] The flaw detection data generation unit 3A continuously acquires the detection signal from the flaw detector 2 at a preset sampling period in synchronization with the relative movement of the flaw detector 2 with respect to the surface of the steel bar 1. The flaw detection data generation unit 3A continuously obtains the maximum output information of each predetermined scanning interval (first partition D1) based on the acquired detection signal, and sequentially stores it in a storage unit such as a database. The above-mentioned detection signal is acquired, for example, for the entire surface of the steel bar 1 to be inspected. The interval of the first partition D1 is predetermined based on the size of the surface defect to be measured. As an example of the interval of the first partition D1, 30 mm can be cited.

[0041] Through the processing of the flaw detection data generating unit 3A, continuous flaw detection data (detection information) is acquired along the scanning direction (flaw detection direction). The continuous flaw detection data includes discrete values ​​in units of preset scanning intervals.

[0042] Hereinafter, a collection of flaw detection data continuously acquired along the surface of the steel bar 1 is referred to as a flaw detection chart 10 .

[0043] The flaw detection diagram 10 can be, for example, Figure 2 Express it that way. Figure 2 2 are exemplified in the flaw detection diagram 10. The horizontal axis represents the scanning direction (flaw detection direction), and the vertical axis represents the maximum value of the output value of the detection signal per predetermined scanning interval (first division D1).

[0044] <Defect Judgment Unit 3B>

[0045] The defect determination unit 3B determines the surface defects based on the flaw detection diagram 10 including the arrangement of the plurality of flaw detection data acquired by the flaw detection data generation unit 3A. Figure 2 As shown, it is determined whether it is greater than a first threshold value TH1 set as a threshold value for determining whether the product is acceptable or not. The first threshold value TH1 is determined in advance as a threshold value capable of determining whether the product is acceptable or not based on the obtained flaw detection data of the steel bar 1 and the state of surface defects of the steel bar product.

[0046] The defect determination unit 3B determines whether the detected output value is less than the first threshold value TH1 for each flaw detection data of the flaw detection diagram 10, for example. Furthermore, when the flaw detection unit 3B detects the flaw detection data determined to be greater than the first threshold value TH1, it performs the following processing. That is, it determines that there is a defect that is a product failure in the area including the flaw detection data, and outputs the information. Figure 2 The examples shown in (a) and (b) illustrate the case where there is a defect of failure.

[0047] In this way, it is determined whether the steel bar 1 to be inspected is acceptable as a product.

[0048] <Defective Property Evaluation Section 3C>

[0049] The defect property evaluation unit 3C performs the following processing based on the characteristics of the data pattern (data map) set based on the arrangement of a plurality of flaw detection data along the surface of the steel bar 1 obtained by flaw detection: That is, it evaluates the properties of the surface defects generated in the steel bar 1 to be inspected.

[0050] Here, the steel bar to be evaluated for the properties of the surface defects is referred to as the evaluated steel bar.

[0051] This evaluation is performed, for example, as follows. The correlation between the properties of the surface defects of the steel bar 1 and the data pattern is obtained in advance, and identification data for identifying the properties of the surface defects is obtained based on the correlation. Then, referring to the identification data obtained in advance, the properties of the surface defects of the steel bar 1 are evaluated based on the characteristics of the obtained data pattern.

[0052] For example, the characteristics of the surface defects of the steel bar 1 are determined by comparing the identification data with the characteristics of the acquired data pattern.

[0053] It should be noted that, in the present embodiment, the plurality of flaw detection data constituting the data pattern are data obtained by flaw detection of the entire surface of the steel bar 1 .

[0054] Next, a first method of the evaluation process of the defect property evaluation unit 3C in the present embodiment will be described.

[0055] In the first method, the following processing is performed on the flaw detection diagram 10 including a set of flaw detection data continuously acquired along the surface of the steel bar 1 generated by the flaw detection data generating unit 3A. Figure 3 As shown, it is determined whether it is greater than the second threshold value TH2 in each first partition D1 (specified scanning interval). That is, it is determined whether each flaw detection data is below the second threshold value TH2. If it is not satisfied, it is considered that there is a surface defect in the first partition D1. Hereinafter, the surface defect is also referred to as the detection defect. In addition, the number of detection defects is referred to as the detection defect number.

[0056] And, in the first method, if Figure 3 and Figure 4 As shown, the surface of the steel bar 1 is divided into a second partition D2 which is larger than the first partition D1. Figure 3 and Figure 4 ), the division direction of the second partition D2 is made the same as the flaw detection direction.

[0057] Then, in the first method, Figure 4 As shown, the defect property evaluation unit 3C first finds the number of first partitions above the second threshold value TH2 in each second partition D2. Next, the flaw detection data is represented by the number of first partitions above the second threshold value TH2 in each second partition D2 (the number of detected defects). That is, the flaw detection data including the defect output is grouped. Then, the flaw detection data is converted into a form represented by the number of detected defects, wherein the number of detected defects includes the number of first partitions above the second threshold value TH2 in each second partition D2.

[0058] In this embodiment, for example, the length (size) of the second partition D2 is an integer multiple of the first partition D1. Figure 3 As shown, the length (size) of the second partition D2 is set to 10 times that of the first partition D1. In this case, the number of detected defects is in the range of 0 to 10. The second partition D2 is preferably set so that each first partition D1 is exclusively included in any second partition D2.

[0059] Next, the defect property evaluation unit 3C extracts the second partition where the number of detected defects is greater than 1. For the extracted second partition, the average value of the number of detected defects in each second partition is obtained and indexed. The index is used as a feature to determine the properties of the surface defects of the steel bar 1. It should be noted that when there is no flaw detection data with a number of detected defects greater than 1, the index is zero. In this specification, the above index is referred to as a defect density index. Figure 4 In the case of the flaw detection diagram 10 shown, the defect density index is 6.0.

[0060] Then, the defect property evaluation unit 3C evaluates the properties of the defects generated in the steel bar 1 to be inspected based on the value of the defect density index obtained.

[0061] For example, the correlation between the properties of the defects and the value of the defect density index is calculated in advance using the flaw detection data of past flaw detection inspections, and the properties of the defects are determined based on the calculated defect density index.

[0062] [Second threshold value TH2]

[0063] Here, the second threshold TH2 is obtained in advance, for example, based on the correlation between the properties of the surface defects of the steel bar 1 and the characteristics of the data pattern obtained in advance. The second threshold TH2 is obtained in advance, for example, as a threshold that can more effectively obtain the flaw detection data (number of detected defects) for classifying the defect properties.

[0064] Alternatively, the second threshold TH2 is determined based on the first threshold TH1. For example, when there are few defective steel bars 1, the second threshold TH2 is set to a value lower than the first threshold TH1. On the other hand, when there are many defective steel bars 1, the second threshold TH2 is set to the value of the first threshold TH1.

[0065] [For the range of indicators used to determine defects]

[0066] The properties of the defects on the surface of the steel bar 1 are, for example, Figure 5 Such types differ depending on the type of defect, the severity of the defect, and the cause of the defect during manufacturing.

[0067] Figure 5 (a) is an example in which a plurality of defects along the length direction are generated over the entire length and circumference of the surface of the steel bar 1. In the following description, such defect properties are referred to as length direction defects 1. When the defect properties are length direction defects 1, the grinding load is very high.

[0068] Figure 5 (b) is an example in which a plurality of defects along the longitudinal direction are generated in a partial region of the surface of the steel bar 1. In the following description, such defect properties are referred to as longitudinal direction defects 2. When the defect properties are longitudinal direction defects 2, the grinding load is high.

[0069] It should be noted that, hereinafter, the longitudinal defect 1 and the longitudinal defect 2 are collectively referred to as the longitudinal defect.

[0070] Figure 5 (c) is an example of a single defect including a crack and a scab. In the following description, such a defect is referred to as a single defect. When the defect is a single defect, the grinding load is low.

[0071] Furthermore, when the defect is characterized by a longitudinal defect 1 or a longitudinal defect 2, as described below, a wider range of grinding is required compared to the case where the defect is characterized by a single defect. As a result, the product may be defective due to the dimensional tolerance being exceeded, and the yield rate may be reduced. Furthermore, the countermeasures for suppressing longitudinal defects are different from those for suppressing single defects.

[0072] Here, Figure 6 The defect characteristics are shown as lengthwise defects 1 ( Figure 6(a)) and lengthwise defects 2 ( Figure 6 (b)), single defect ( Figure 6 An example of flaw detection diagram 10 of case (c)). Figure 5 An example of a defect in the longitudinal direction at this time is shown.

[0073] like Figure 6 As shown, the length direction defect is greatly increased compared with the single defect.

[0074] in addition, Figure 7 The defect characteristics are shown as lengthwise defects 1 ( Figure 7 (a)) and lengthwise defects 2 ( Figure 7 (b)), single defect ( Figure 7 Another example of flaw detection diagram 10 of case (c)).

[0075] like Figure 7 As shown in (a), in the case of a lengthwise defect of 1, the defect output value is generally high. Figure 7 As shown in (b), in the case of a longitudinal defect 2, the defect output value is high in a local area. Figure 7 As shown in (c), a single defect is manifested as a high value of a single defect output value.

[0076] As described above, the inventors of the present application believe that the properties of the defect are correlated with the properties (pattern of the diagram) of the flaw detection diagram 10. Furthermore, the inventors of the present application believe that the correlation should be expressed as an index.

[0077] Next, an attempt was made to perform statistical evaluation on the flaw detection diagrams 10 of a plurality of past steel bars 1 and the properties of the defects at that time.

[0078] Table 1 shows the results when the defect type is defect 1 in the longitudinal direction.

[0079] [Table 1]

[0080] Maximum 36.0 average value 30.2 σ 3.3 Mean + σ 33.4

[0081] Table 2 shows the results when the defect type is defect 2 in the longitudinal direction.

[0082] [Table 2]

[0083] Maximum 36.3 average value 13.4 σ 5.9 Mean + σ 19.3

[0084] Table 3 shows the results when the defect characteristics are single defects.

[0085] [Table 3]

[0086] Maximum 36.9 average value 10.7 σ 3.5 Mean + σ 14.2

[0087] Tables 1 to 3 are tables for obtaining the maximum value, average value, etc. of the data for the flaw diagram 10 of the flaw data including the defect output value. As can be seen from Tables 1 to 3, the properties of the defect cannot be effectively evaluated at the maximum value of the defect. On the other hand, when the average value or average value + σ of the output value of the flaw diagram 10 is used as an index, the properties of the defect can be evaluated by the average value or average value + σ. It should be noted that the present disclosure also includes the case where the average value or average value + σ of the data obtained from the flaw diagram 10 itself is used as an index to evaluate the properties of the defect.

[0088] However, in the example of defect properties such as shown in Table 4, when the above-mentioned "average value + σ" is used as an index as described in Table 4, it is impossible to distinguish between a longitudinal defect and a single defect.

[0089] [Table 4]

[0090]

[0091] Therefore, in this embodiment, the purpose is to improve the accuracy of distinction. Figure 3 and Figure 4 As shown in FIG. 1 , each flaw detection data of the flaw detection diagram 10 is grouped into units of the second partition D2 wider than the first partition D1. Then, the average value of the number of defects existing in each second partition D2 is obtained as the defect density index as described above. However, only the second partition D2 with defects is taken as the object, and the average value of the number of defects is obtained as an index (feature amount) representing the characteristics of the property (pattern) of the flaw detection diagram 10.

[0092] If the defect density index is used, then Figure 6 As shown in Table 4, it can be seen that the longitudinal defects and single defects can be distinguished more clearly.

[0093] In the present embodiment, as the index range, the case where the defect concentration index is 3 to 10 is evaluated as a longitudinal defect. In addition, the case where the defect concentration index is less than 3 (greater than 0) is evaluated as a single defect.

[0094] (Operation and others)

[0095] In the present embodiment, flaw detection is performed along the surface of the steel bar 1 using the flaw detector 2 of the flaw detection device.

[0096] Using the flaw detection image 10 obtained by the flaw detection and the first threshold value TH1 set in advance, it is determined whether there is a defect that makes the product unacceptable (see Figure 2 ). It should be noted that the first threshold TH1 is set to a different value depending on the quality required for the product.

[0097] Furthermore, in the present embodiment, the properties of defects generated in the steel bar 1 are evaluated based on the flaw detection data. That is, in the present embodiment, it is not necessary to directly observe the state of defects on the surface of the steel bar 1 to evaluate the properties of the defects. Furthermore, based on the graph (data pattern) of the flaw detection data used for defect detection, the properties of defects generated in the steel bar 1 can be evaluated for all the manufactured steel bars 1.

[0098] It should be noted that the evaluation of the properties of the defects may be performed only on the steel bar 1 which is a defective product.

[0099] At this time, in this embodiment (first method), in order to evaluate the properties of the defects, the flaw map 10 (array of flaw detection data) containing the output values ​​of the detection is processed as follows. That is, it is transformed into a flaw map 10 containing an array of flaw detection data formed by the number of defects. Then, as a feature of the data pattern (property) of the transformed flaw map 10, a defect density index containing an average value is calculated and the flaw map 10 is indexed. Next, the properties of the defects are evaluated by the defect density index. As a result, in this embodiment, it is possible to distinguish between longitudinal defects and single defects more clearly and simply.

[0100] Furthermore, the properties of defects generated in each steel bar 1 can be evaluated based on the flaw detection data without actually visually checking each steel bar 1. Therefore, the tendency of defects generated during the production of the steel bar 1 can be automatically and quickly evaluated.

[0101] Furthermore, the manufacturing conditions for manufacturing the steel bar 1 may be optimized in conjunction with the generated defects.

[0102] Here, if Figure 5 As shown, in order to remove the defects of the longitudinal defects, a wider range of grinding is required than that of the single defects. The optimal conditions for heating and rolling when manufacturing the steel bar 1 for suppressing the longitudinal defects are different from the optimal conditions for heating and rolling when suppressing the single defects.

[0103] As described above, in the present embodiment, by evaluating the properties of defects and optimizing the manufacturing conditions for manufacturing the steel bar 1, it is possible to significantly reduce the steel bar 1 in which defects that constitute product failures occur. As a result, the yield rate is improved.

[0104] In addition, compared with longitudinal defects, single defects are more likely to become acceptable products through grinding. Since the present embodiment can easily sort out the steel bars 1 with single defects from among the unacceptable steel bars 1, this aspect also contributes to an improvement in yield.

[0105] (Variation Example)

[0106] (1) In the above embodiment, an example is given in which the defect properties are divided into two properties (longitudinal defects and single defects). However, the index range may be set so as to be divided into three or more properties.

[0107] (2) In the above description, the average value (defect density index) is obtained as an index after extracting the order of arrangement of the transformed flaw detection data (number of defects), and the defect density index is used as an index representing the characteristics of the data pattern to determine the nature of the defect.

[0108] The characteristics of the data pattern can also be obtained by considering the order of arrangement of the flaw detection data. For example, the longitudinal defects have the characteristic that defects of a predetermined size or above appear continuously in the longitudinal direction. The characteristics of the data pattern can also be obtained based on the dependence of the defects generated along the longitudinal direction of such longitudinal defects.

[0109] (3) In the above embodiment, the flaw detection data including the detection output value is converted into the flaw detection data consisting of the number of defects. Then, the properties of the defects are evaluated based on the characteristics of the properties (data pattern) of the flaw detection diagram 10 .

[0110] The properties of the defects may be evaluated based on the features in the arrangement (data pattern) of the flaw detection data including the output values ​​of the detected defects.

[0111] (4) As a second method for evaluating the properties of defects, the properties of defects may be evaluated using machine learning.

[0112] For example, the properties of surface defects detected in the past are classified into two or more types, and the data of the flaw detection diagram 10 of the steel bar 1 are associated with the properties of each surface defect to perform machine learning. Then, referring to the machine learning results, it is evaluated which defect property the obtained flaw detection diagram 10 is.

[0113] (5) It should be noted that the classification of defect characteristics is preferably carried out in association with the causes of the defects.

[0114] (other)

[0115] The present disclosure may also adopt the following configurations.

[0116] (1) A surface defect evaluation method for evaluating the properties of surface defects of a steel bar, wherein:

[0117] The correlation between the properties of the surface defects of the steel bar and the characteristics of the data pattern obtained by flaw detection along the surface of the steel bar is obtained in advance.

[0118] The properties of the surface defects of the steel bar to be evaluated are determined based on the above correlation and the characteristics of the data pattern obtained by flaw detection on the steel bar to be evaluated. The steel bar to be evaluated is a steel bar for which the properties of the surface defects are evaluated.

[0119] (2) The characteristics of the data pattern are set based on the arrangement of a plurality of flaw detection data along the surface of the steel bar obtained by the flaw detection.

[0120] (3) The characteristics of the above data pattern are indexed and the properties of the surface defects of the steel bar are evaluated using the index.

[0121] (4) dividing the surface of the steel bar into a plurality of first partitions along the flaw detection direction, and determining whether the flaw detection data of each first partition is above a preset threshold value;

[0122] The surface of the steel bar is divided into a second partition larger than the first partition along the surface of the steel bar.

[0123] Find the number of first partitions above the threshold value in each second partition.

[0124] The characteristics of the data pattern are indexed based on the number of detected defects including the number of first partitions that are above the threshold.

[0125] (5) extracting the second partitions in which the number of detected defects is 1 or more, and taking the average value of the number of detected defects of each of the extracted second partitions as the feature of the data pattern.

[0126] (6) The plurality of flaw detection data constituting the data pattern include flaw detection data obtained by flaw detection of the entire surface of the steel bar.

[0127] The entire contents of Japanese Patent Application 2022-057151 (filed on March 30, 2022) to which this application claims priority are incorporated herein by reference as a part of this disclosure. Here, the invention is described with reference to a limited number of embodiments, but the scope of rights is not limited thereto, and changes to the embodiments based on the above disclosure are obvious to those skilled in the art.

[0128] Description of Reference Numerals

[0129] 1 Steel bar

[0130] 2 Flaw detector

[0131] 3. Flaw Detection Control Department

[0132] 3A Flaw Detection Data Generation Department

[0133] 3B Defect Assessment Department

[0134] 3C Defect Characteristic Evaluation Department

[0135] 10 Flaw detection diagram

[0136] TH1 1st threshold

[0137] TH2 Second Threshold

[0138] D1 Division 1

[0139] D2 Division 2

Claims

1. A method for evaluating surface defects of a steel bar, wherein the properties of surface defects of the steel bar are evaluated, wherein: The correlation between the properties of the surface defects of the steel bar and the characteristics of the data pattern obtained by flaw detection along the surface of the steel bar is obtained in advance. The properties of the surface defects of the evaluated steel bar are determined based on the correlation and the characteristics of the data pattern obtained by flaw detection on the evaluated steel bar, which is the steel bar for which the properties of the surface defects are evaluated.

2. The method for evaluating surface defects of a steel bar according to claim 1, wherein: The characteristics of the data pattern are set based on the arrangement of a plurality of flaw detection data along the surface of the steel bar acquired by the flaw detection.

3. The method for evaluating surface defects of a steel bar according to claim 1 or 2, wherein: The characteristics of the data pattern are indexed, and the properties of the surface defects of the steel bar are evaluated by the index.

4. The method for evaluating surface defects of a steel bar according to claim 3, wherein: The surface of the steel bar is divided into a plurality of first partitions along the flaw detection direction, and it is determined whether the flaw detection data of each first partition is above a preset threshold value. The surface of the steel bar is divided into a second partition larger than the first partition along the surface of the steel bar, Find the number of first partitions above the threshold value in each second partition. The characteristics of the data pattern are indexed based on the number of detected defects including the number of first partitions that are greater than a threshold value.

5. The method for evaluating surface defects of a steel bar according to claim 4, wherein: The second partitions having the number of detected defects being 1 or more are extracted, and for the extracted second partitions, an average value of the number of detected defects per second partition is used as a feature of the data pattern.

6. The method for evaluating surface defects of a steel bar according to any one of claims 2 to 5, characterized in that: The plurality of flaw detection data constituting the data pattern include flaw detection data obtained by flaw detection of the entire surface of the steel bar.