Zein-citrus pectin nanoparticles loaded with prodigiosin and preparation method of zein-citrus pectin nanoparticles
The preparation of nanoparticles loaded with zein and citrus pectin by combining zein and citrus pectin, solves the problems of insoluble in water and easy decomposition, improves its stability and embedding rate, and ensures that it is in medicine safe and effective application in the field.
Patent Information
- Application Number
- CN202410955392.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-07-17
AI Technical Summary
Lymphin is insoluble in water and easy to decompose, which limits its application in the pharmaceutical field, especially as a potential use as an antibacterial and anticancer drug.
The nanoparticles loaded with zein and citrus pectin are prepared by combining zein and citrus pectin. The nanoparticles are embedded with zein and modified and stabilized with citrus pectin to form a core-shell structure. To improve stability.
Improve the stability and water solubility of lycopene, protect it from being damaged and decomposed by the external environment, significantly improve the embedding rate and stability in adverse environments, and ensure its safety and effectiveness in practical applications. .
Smart Images

Figure CN118985898A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of food functional compounds and biomedicine, and in particular to prodigiosin-loaded zein-citrus pectin nanoparticles and a preparation method thereof. Background Art
[0002] Prodigiosin is a natural red pigment produced by microorganisms, which can be produced by microorganisms such as Serratia, Riveria, and Pseudomonas. Its structure is a tripyrrole ring structure, which is soluble in organic solvents such as methanol and ethanol, and is insoluble in water. The strain used in the present invention is Serratia marcescens. The pigment has antibacterial, anticancer, anti-inflammatory and other biological activities, and has a wide range of application prospects in the medical field, food field, etc. In the medical field, prodigiosin can be used as a potential anticancer and antimalarial drug, and in the food field, it can be used as a potential colorant or preservative with antibacterial activity. The most studied is the biological activity of prodigiosin in the medical field, among which the antibacterial activity and anticancer activity of prodigiosin are the key points and focus of research at home and abroad.
[0003] Zein is a protein extracted from corn endosperm. It is insoluble in water and belongs to alcohol-soluble protein. However, it lacks essential amino acids such as lysine and tryptophan. Zein has low nutritional value, which limits its application. Zein has been approved by the US Food and Drug Administration (FDA) as a generally recognized as safe (GRAS) pharmaceutical excipient. Since zein has hydrophobic regions and is easy for small molecules to self-assemble, zein can be used to encapsulate bioactive substances and has the potential to be used as a nanocarrier. However, single zein nanoparticles are unstable. Zein tends to be unstable and aggregate under high salt, high heat or pH values near the isoelectric point. The main way to solve these problems is to add some stabilizers such as hydrophilic polysaccharides.
[0004] Citrus pectin is a natural anionic polysaccharide widely found in plant cell walls. It is a hydrophilic natural polymer with multiple functional properties. It is usually used as a thickener, stabilizer, gelling agent and delivery carrier, and is widely used in the fields of food and medicine. Pectin is mainly a class of acidic heteropolysaccharides composed of D-galacturonic acid (D-Gal-A) connected by α-1,4-glycosidic bonds. In addition to D-Gal-A, it also contains neutral sugars such as L-rhamnose, D-galactose, and D-arabinose. Zein-citrus pectin composite nanoparticles have the advantages of being green, safe, and low-cost, and have potential application prospects. At present, there are no reports on zein-citrus pectin nanoparticles loaded with prodigiosin. Summary of the invention
[0005] The object of the present invention is to provide a zein-citrus pectin nanoparticle loaded with prodigiosin and a preparation method thereof. The present invention utilizes alcohol-soluble zein and hydrophilic pectin to prepare zein-citrus pectin nanoparticles of prodigiosin by mixing the alcohol-soluble zein and hydrophilic pectin with prodigiosin. The process conditions of the present invention solve the solubility problem of prodigiosin in water in application and the problem of prodigiosin being easy to decompose, thereby promoting the application of prodigiosin in the field of medicine.
[0006] The present invention is achieved through the following technical solutions: A prodigiosin-loaded zein-citrus pectin nanoparticle, characterized in that the structure of the nanoparticle is a core-shell structure with zein as a core and citrus pectin as a shell, the prodigiosin enters the hydrophobic cavity of the zein, and the citrus pectin is wrapped on the surface of the zein.
[0007] The present invention also provides a method for preparing the prodigiosin-loaded zein-citrus pectin nanoparticles, comprising the following steps: S1, dissolving zein in 80% (V / V) ethanol aqueous solution to obtain a zein stock solution; S2, adding prodigiosin to the above zein stock solution, stirring with a magnetic stirrer to fully dissolve the zein and prodigiosin, and adjusting the pH to 4.0 with a 0.1M HCl solution to obtain a zein-prodigiosin ethanol solution; S3, dissolving citrus pectin in ultrapure water to obtain a citrus pectin stock solution; S4, slowly adding the zein-prodigiosin ethanol solution obtained in S2 to ultrapure water with a pH of 4.0, mixing and stirring to obtain a dispersion of zein nanoparticles loaded with prodigiosin; performing reduced pressure heating and rotary evaporation to remove ethanol, and then replenishing the dispersion to the original volume with ultrapure water; S5, slowly dropwise adding the dispersion obtained in S4 into the citrus pectin solution, mixing and stirring to obtain a dispersion of zein-citrus pectin nanoparticles loaded with prodigiosin, and storing the dispersion at 4° C. away from light; S6. The dispersion of S5 was centrifuged at low speed to remove aggregates, and the supernatant was freeze-dried to obtain zein-citrus pectin nanoparticles loaded with prodigiosin.
[0008] Furthermore, in step S1, the concentration of the zein stock solution is 5 g / L.
[0009] Furthermore, in step S2, the rotation speed of the magnetic stirring is 600 rpm and the time is 1 hour.
[0010] Furthermore, the mass ratio of zein to prodigiosin in the zein-prodigiosin ethanol solution is 10:1.
[0011] Furthermore, the specific operation of step S3 is as follows: dissolving citrus pectin in ultrapure water, stirring in a water bath at 65° C. and 600 rpm for 1 hour, cooling to room temperature, and adjusting the pH to 4.0 with 0.1 M HCl solution to obtain a citrus pectin stock solution.
[0012] Furthermore, the concentration of citrus pectin in step S3 is 2 g / L.
[0013] Furthermore, the conditions for the reduced pressure rotary evaporation in step S4 are a pressure of -0.1 MPa, a temperature of 45° C., and evaporation for 15 minutes.
[0014] Furthermore, in step S4, the volume ratio of the zein nanoparticle dispersion loaded with prodigiosin, zein-prodigiosin ethanol solution, to ultrapure water is 1:4.
[0015] Furthermore, in step S5, the mass ratio of zein to citrus pectin is 20:1-1:1, the speed of magnetic stirring is 600 rpm, and the time is 1 hour.
[0016] Furthermore, the centrifugal conditions in step S6 are: a rotation speed of 4000 rpm and a time of 10 min; and the freeze-drying conditions are: a temperature of -45°C and a time of 72 h.
[0017] Beneficial technical effects of the present invention: The invention uses the strong hydrophobicity of zein to embed prodigiosin into the hydrophobic cavity of the zein, and then uses hydrophilic citrus pectin to modify, embed and stabilize nanoparticles, thereby improving the stability of the nanoparticles. The zein-citrus pectin nanoparticles loaded with prodigiosin prepared by the invention improve the stability and solubility of prodigiosin in water, and can protect prodigiosin from being destroyed and decomposed by the external environment. At present, there is no report on the zein-citrus pectin nanoparticles loaded with prodigiosin.
[0018] The fluorescence spectrum, surface hydrophobicity and Fourier infrared transform spectrum of the zein-citrus pectin nanoparticles loaded with prodigiosin prepared by the present invention show that the two are combined, prodigiosin enters the hydrophobic cavity of zein, and citrus pectin is wrapped on the surface of zein to form nanoparticles with zein as the core and citrus pectin as the shell structure, which has a high embedding rate for prodigiosin and still has excellent stability under adverse environments. The zein-citrus pectin nanoparticles loaded with prodigiosin prepared by the present invention present spherical particles with uniform size and smooth surface in the structural characterization scanning electron microscope.
[0019] The process of the invention solves the solubility problem and easy decomposition problem of prodigiosin being insoluble in water. The fact that prodigiosin is insoluble in water but easily soluble in organic solvents hinders its application. The invention adopts bio-based materials as nanoparticle wall materials to ensure the safety of prodigiosin in practical applications.
[0020] The method for preparing the prodigiosin-loaded zein-citrus pectin nanoparticles prepared in the present invention is simple to operate, requires few equipments, is green and safe, has low cost, and has good biocompatibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 The potential distribution diagram of the zein-Pet / PG nanoparticles loaded with prodigiosin obtained in Example 1 and the zein-PG nanoparticles loaded with prodigiosin obtained in Comparative Example 1; Figure 2 The particle size distribution diagram of the zein-Pet / PG nanoparticles loaded with prodigiosin obtained in Example 1 and the zein-PG obtained in Comparative Example 1; Figure 3 The scanning electron microscope images of the zein-Pet / PG nanoparticles loaded with prodigiosin at different zein-citrus pectin mass ratios and the zein-PG obtained in Comparative Example 1; Figure 4 The fluorescence spectra of the prodigiosin-loaded zein-Pet / PG nanoparticles obtained in Example 1 and the zein-PG obtained in Comparative Example 1 are shown in FIG. Figure 5 This is a surface hydrophobicity performance diagram of the zein-citrus pectin nanoparticles loaded with prodigiosin, i.e., zein-Pet / PG2:1, obtained when the mass ratio of zein-citrus pectin is 2:1, and the zein-PG obtained in Comparative Example 1.
[0022] Figure 6 Fourier transform infrared spectra of citrus pectin, prodigiosin and zein; Figure 7 Fourier transform infrared spectra of zein-prodigiosin nanoparticles and zein-Pet / PG2:1; Figure 8 This is the effect of pH on the particle size of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig. 9 This is the effect of pH on the potential of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig.10This is the effect of NaCl on the particle size of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig.11 This is the effect of NaCl on the potential of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig.12 This is the effect of ultraviolet light on the retention rate of prodigiosin in free prodigiosin, zein-PG, and zein-Pet / PG2:1 nanoparticles. DETAILED DESCRIPTION
[0023] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0024] Example 1 A method for preparing zein-citrus pectin nanoparticles loaded with prodigiosin, comprising the steps of: (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0025] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour, and obtain a zein stock solution with a concentration of 5 g / L.
[0026] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0027] (4) Preparation of citrus pectin solution 2.0 g of citrus pectin was dissolved in 100 mL of ultrapure water, heated and stirred at 600 rpm and 65° C. for 1 h, cooled to room temperature, and the pH was adjusted to 4.0 with 0.1 M NaOH solution to obtain a citrus pectin stock solution.
[0028] (5) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0029] (6) Adding the solution obtained in (5) to the citrus pectin solution, wherein the amount of citrus pectin added is 50 mg, 25 mg, 10 mg, 5 mg, and 2.5 mg, respectively, and mixing and stirring to obtain a dispersion of zein-citrus pectin nanoparticles loaded with prodigiosin, which is then stored at 4° C. away from light; (7) The dispersion obtained in (6) was centrifuged at 4000 rpm for 10 min, and a portion of the supernatant was stored at 4°C for subsequent research; a portion of the supernatant was freeze-dried at -45°C for 72 h to obtain zein-citrus pectin nanoparticle powder loaded with prodigiosin.
[0030] Comparative Example 1 (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0031] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour to obtain a 5 g / L zein stock solution.
[0032] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0033] (4) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0034] (5) The dispersion obtained in (4) was centrifuged at 4000 rpm for 10 min, and a portion of the supernatant was stored at 4°C for subsequent research; a portion of the supernatant was freeze-dried at -45°C for 72 h to obtain zein nanoparticle powder loaded with prodigiosin.
[0035] Data Characterization: The nanoparticles prepared in the above Example 1 and Comparative Example 1 were tested, and the specific test contents were as follows: 1. If Figure 1 As shown, Figure 1-2 It is the particle size potential distribution diagram of Example 1 and Comparative Example 1. The zein-citrus pectin nanoparticles loaded with prodigiosin prepared in Example 1 are negatively charged in a solution of pH 4.0, wherein zein is positively charged and citrus pectin is negatively charged, and the two substances are oppositely charged and combined by electrostatic attraction. As the mass ratio of zein to citrus pectin changes, the corresponding nanoparticles have different charges. When the amount of citrus pectin added increases, the charge carrying amount of the nanoparticles also increases, and its ζ-potential gradually decreases. When the amount of citrus pectin added is 2.5 mg, that is, the mass ratio of zein to citrus pectin is 20:1, citrus pectin is not enough to wrap zein, and the low electrostatic attraction causes the nanoparticles to aggregate into precipitation, and no subsequent particle size test is performed. The particle size of Zein-Pet / PG nanoparticles is 184-326nm, the PDI is less than 0.3, and the ζ-potential value is less than -20mV, indicating that the prepared nanoparticles have a small particle size, a negatively charged surface, and good dispersibility. In Example 1, the particle size of zein-Pet / PG2:1 nanoparticles is the smallest, and the particle size of zein-Pet / PG20:1 nanoparticles is the largest.
[0036] In the solution of pH 4.0, the zein-prodigiosin nanoparticles prepared in Comparative Example 1 have a positive charge, a ζ-potential of 23.6 mV, a particle size of 121.6 nm, and a PDI of 0.353, because the pH value is lower than the isoelectric point of zein. The nanoparticles prepared by this method have a smaller particle size, a negative charge on the surface, and a larger PDI, which may be due to the strong hydrophobicity of zein, and it is difficult to form uniform nanoparticles during the self-assembly process.
[0037] 2. As shown in Table 1, Table 1 is the embedding rate and loading rate of prodigiosin in Example 1 and Comparative Example 1. In Comparative Example 1, the embedding rate of prodigiosin by zein-PG nanoparticles without adding citrus pectin is 46.46%, indicating that a part of prodigiosin is not encapsulated in the nanoparticles during the preparation process, or leaks out after the nanoparticles are formed. In Example 1, after adding citrus pectin, the embedding rate of prodigiosin by the nanoparticles is 65.83~89.05%. The encapsulation rate of prodigiosin by the nanoparticles prepared by this method is significantly higher than that of the nanoparticles in Comparative Example 1, which indicates that the presence of citrus pectin prevents prodigiosin from leaking from zein and improves its embedding rate. The zein-Pet / PG2:1 nanoparticles show the highest prodigiosin encapsulation rate, up to 89.05%, indicating that citrus pectin provides electrostatic repulsion and spatial repulsion, making the nanoparticle structure more stable.
[0038]
[0039] 3. If Figure 3 As shown, Figure 3 The scanning electron microscope images of Example 1 and Comparative Example 1. The zein-PG nanoparticles are distributed in a spherical shape, but their surface is relatively rough. In addition, the nanoparticles are interconnected and in a clump shape. After adding citrus pectin, the Z-Pet / PG nanoparticles are also distributed in a spherical shape, and their surface is smoother than that of the zein-PG nanoparticles, and their shape distribution is more regular. When citrus pectin is added in excess, the Z-Pet / PG1:1 nanoparticles are cross-linked with each other, and the excess citrus pectin increases the viscosity of the nanoparticle surface. When the amount of citrus pectin added is small, the Z-Pet / PG10:1 nanoparticles are uneven in size. Due to the lack of citrus pectin, the electrostatic repulsion between the nanoparticles is weak, and the nanoparticles aggregate. When the mass ratio of zein to citrus pectin is 2:1, the nanoparticles are uniform in size. The SEM results are consistent with the dynamic light scattering particle size distribution trend, but the dynamic light scattering measures the hydrated particle size, while the SEM is the particle size of the freeze-dried nanoparticles. Therefore, the nanoparticle size in the SEM is smaller than that in the DLS.
[0040] 4. If Figure 4 As shown, Figure 4The fluorescence spectra of Example 1 and Comparative Example 1 at an excitation wavelength of 280 nm and an emission wavelength of 290-450 nm are shown. After excitation at 280 nm, the zein nanoparticles show a fluorescence emission spectrum in the range of 290-450 nm, with an emission peak at 303 nm, which is due to the presence of tyrosine residues in the zein molecule. The tyrosine residues in the protein will show a typical fluorescence emission peak near 304 nm after excitation at 280 nm. After adding pectin, the maximum emission wavelength of zein did not change significantly, but its fluorescence intensity at 303 nm was significantly reduced, indicating that pectin quenched the intrinsic fluorescence of zein, which may be due to the interaction of negatively charged pectin with positively charged tyrosine residues (pI of 5.66) through electrostatic attraction, resulting in fluorescence quenching.
[0041] 5. The surface hydrophobicity of the composite nanoparticles was determined by the ANS probe method to further study the interaction between zein and pectin. Figure 5 The surface hydrophobicity index of the zein-citrus pectin nanoparticles loaded with prodigiosin, i.e., zein-Pet / PG2:1, obtained when the mass ratio of zein-citrus pectin was 2:1, and the zein-PG obtained in Comparative Example 1. Due to the presence of more hydrophobic amino acid residues in zein, the zein-PG nanoparticles showed high surface hydrophobicity, and showed extremely high SHI (251510 and 227100) at pH 3.0 and 4.0. After adding pectin, the SHI of Z-Pet / PG2:1 nanoparticles decreased, dropping sharply to 59133 and 58317 at pH 3.0 and pH 4.0, respectively, indicating that the added pectin affected the binding between ANS and the surface of zein nanoparticles. Pectin embedded the hydrophobic groups on the surface of zein through interaction forces such as electrostatic attraction, thereby blocking the available hydrophobic areas for zein to bind to ANS, reducing the electrostatic force of zein binding to ANS, and improving its stability in aqueous solution.
[0042] 6. If Figure 6-7 As shown, Figure 6 Fourier transform infrared spectra of citrus pectin, prodigiosin and zein; Figure 7 The Fourier transform infrared spectra of zein-prodigiosin nanoparticles and zein-Pet / PG2:1 are shown in Figure 1. The FTIR spectrum of zein is at 3279.7, 1636.2 and 1514.5 cm -1 The FTIR spectrum of citrus pectin shows typical absorption peaks at 3397.1, 1734.8, 1084.1, and 1012.3 cm-1, which are related to O–H stretching vibration, amide I band (C=O stretching vibration), and amide II band (C–N stretching vibration and N–H bending vibration).-1 The characteristic absorption peaks are shown at 3397.1 and 1734.8 cm -1 They are generated by O–H stretching vibration and C=O stretching vibration respectively. The FTIR spectrum of prodigiosin is 3397.1, 2922.4, 2853.6, 1730.4, 1556.5, 1465.2, 1371.0, 1238.4, 1097.1 cm -1 Characteristic absorption peaks are shown at 3397.1cm -1 , mainly related to NH stretching, 2922.4cm -1 The faint peak at 1097.1 cm is CH (methyl, methylene and methylene) stretching. -1 The strong peaks at are CO and CN stretching.
[0043] The O–H stretching vibration absorption band of zein (3284.3 cm -1 ) compared with the zein-PG nanoparticles, the O–H stretching vibration absorption band shifted to 3291.8 cm -1 , indicating that the amide groups of zein interact with prodigiosin to form hydrogen bonds; when pectin is added, the OH stretching band moves to 3282.6 cm -1 , indicating that there is a strong hydrogen bond between the -OH groups in pectin and the glutamine groups in zein. In addition, the 1636.2 and 1514.5 cm -1 The absorption peaks of amide I band (C=O stretching vibration) and amide II band (C–N stretching vibration and N–H bending vibration) in zein are located at 1644.9 cm-1. After the addition of prodigiosin, the absorption peaks of amide I and amide II bands of zein-PG nanoparticles migrate to 1644.9 cm-1, respectively. -1 and 1528.2cm -1 , indicating that there is a hydrophobic interaction between zein and PG. After adding pectin, the absorption peaks of amide I and amide II of Z-Pet / PG2:1 migrated to 1639.1 cm -1 and 1531.1cm -1 , indicating that there are hydrogen bonds, electrostatic interactions and hydrophobic interactions among the three. In summary, the changes in the FTIR spectrum show that there are not only hydrophobic interactions, but also hydrogen bonds and electrostatic interactions among the three.
[0044] Example 2 A method for preparing zein-citrus pectin nanoparticles loaded with prodigiosin, comprising the steps of: (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0045] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour, and obtain a zein stock solution with a concentration of 5 g / L.
[0046] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0047] (4) Preparation of citrus pectin solution 2.0 g of citrus pectin was dissolved in 100 mL of ultrapure water, heated and stirred at 600 rpm and 65° C. for 1 h, cooled to room temperature, and the pH was adjusted to 4.0 with 0.1 M NaOH solution to obtain a citrus pectin stock solution.
[0048] (5) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0049] (6) Adding the solution obtained in (5) to the citrus pectin solution, wherein the amount of citrus pectin added is 50 mg, 25 mg, 10 mg, 5 mg, and 2.5 mg, respectively, and mixing and stirring to obtain a dispersion of zein-citrus pectin nanoparticles loaded with prodigiosin, which is then stored at 4° C. away from light; (7) The dispersion obtained in (6) was centrifuged at 4000 rpm for 10 min, and the pH of the supernatant was adjusted to 2-7 with 0.1 M HCl or NaOH to obtain zein-citrus pectin nanoparticle dispersions loaded with prodigiosin at different pH values.
[0050] Comparative Example 2 (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0051] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour, and obtain a zein stock solution with a concentration of 5 g / L.
[0052] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0053] (4) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0054] (5) The dispersion obtained in (4) was centrifuged at 4000 rpm for 10 min, and the pH of the supernatant was adjusted to 2-7 with 0.1 M HCl or NaOH to obtain prodigiosin-loaded zein nanoparticle dispersions with different pH values.
[0055] Compared with Comparative Example 1, the pH of the zein nanoparticle dispersion loaded with prodigiosin in Comparative Example 2 is 2-7.
[0056] Data characterization of Comparative Example 2 and Example 2: 1. If Figure 8-9 As shown, Figure 8 This is the effect of pH on the particle size of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig. 9The effect of pH on the potential of zein-PG and zein-Pet / PG2:1 nanoparticles; the data show that when the pH is 5 and 6, the zein-PG nanoparticles are unstable and aggregated and precipitated. Citrus pectin is negatively charged at pH 2-7. When the pH value drops from 7.0 to 2.0, the ζ-potential of citrus pectin gradually increases from -29.0mV to -3.1mV, and the static charge gradually decreases. The particle size of Z-Pet / PG2:1 nanoparticles is about 180nm at pH 3.0-7.0, and the particle size increases to 309.33nm at pH 2.0. When the pH value is 2.0, the ζ-potential of the nanoparticles is close to 0mV. This is because the pKa value of pectin is close to 3. The protonation of the anionic carboxyl groups on pectin and zein leads to a decrease in the net charge of the outer layer, a weakening of the electrostatic repulsion, and an increase in the particle size of the nanoparticles. In addition, the ζ-potential of Zein-Pet / PG2:1 nanoparticles gradually increased from -28.0mV to -2.2mV, and its potential showed a similar trend of change as that of citrus pectin, indicating that citrus pectin was wrapped on the surface of zein through intermolecular forces and spatial repulsion to form stable nanoparticles. Zein-Pet / PG2:1 nanoparticles showed good stability in the pH range of 3.0-7.0, without aggregation, indicating that pH had little effect on Zein-Pet / PG2:1 nanoparticles.
[0057] Example 3 (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0058] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour, and obtain a zein stock solution with a concentration of 5 g / L.
[0059] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0060] (4) Preparation of citrus pectin solution 2.0 g of citrus pectin was dissolved in 100 mL of ultrapure water, heated and stirred at 600 rpm and 65° C. for 1 h, cooled to room temperature, and the pH was adjusted to 4.0 with 0.1 M NaOH solution to obtain a citrus pectin stock solution.
[0061] (5) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0062] (6) Adding the solution obtained in (5) to the citrus pectin solution, wherein the amount of citrus pectin added is 50 mg, 25 mg, 10 mg, 5 mg, and 2.5 mg, respectively, and mixing and stirring to obtain a dispersion of zein-citrus pectin nanoparticles loaded with prodigiosin, which is then stored at 4° C. away from light; (7) The dispersion obtained in (6) was centrifuged at a low speed of 4000 rpm for 10 min, and the supernatant was adjusted to a final salt ion concentration of 0-100 mM with NaCl to obtain zein-citrus pectin nanoparticle dispersions loaded with prodigiosin at different salt ion concentrations.
[0063] Compared with Example 1, the salt ion concentration of the prodigiosin-loaded zein-citrus pectin nanoparticle dispersion of Example 3 is 0-100 mM.
[0064] Comparative Example 3 (1) Extraction of prodigiosin Prodigiosin is obtained from the fermentation of Serratia marcescens. The fermentation liquid of Serratia marcescens is centrifuged to discard the supernatant, the bacteria are extracted with acidified ethanol (pH 3.5), the supernatant is retained by centrifugation, the ethanol is removed by rotary evaporation, and the crude extract of prodigiosin is obtained after drying.
[0065] (2) Preparation of zein solution Weigh 1.0 g of zein, dissolve the zein powder in 200 mL of 80% ethanol solution, stir at 600 rpm for 1 hour, and obtain a zein stock solution with a concentration of 5 g / L.
[0066] (3) Preparation of mixed solution of prodigiosin and zein Weigh 0.1 g of prodigiosin and add it to the above zein solution. Stir thoroughly at 600 rpm for 1 h. Adjust the pH to 4.0 with 0.1 M HCl solution to obtain a zein prodigiosin stock solution.
[0067] (4) 10 mL of the zein prodigiosin stock solution prepared in step (3) was added dropwise to 40 mL of ultrapure water having a pH of 4.0. The mixture was stirred at 600 rpm for 1 h and the ethanol in the mixed solution was removed by rotary evaporation. The conditions for the reduced pressure rotary evaporation were a pressure of -0.1 MPa and a temperature of 45°C for 15 min. The mixture was then filled to 50 mL with an appropriate amount of ultrapure water.
[0068] (5) The dispersion obtained in (4) was centrifuged at a low speed of 4000 rpm for 10 min, and the supernatant was adjusted to a final salt ion concentration of 0-100 mM with NaCl to obtain dispersions of zein nanoparticles loaded with prodigiosin with different salt ion concentrations.
[0069] Compared with Comparative Example 1, the salt ion concentration of the zein nanoparticle dispersion loaded with prodigiosin in Comparative Example 3 is 0-100 mM.
[0070] Data characterization of Comparative Example 3 and Example 3: (1) If Figure 10-11 As shown, Fig.10 This is the effect of NaCl on the particle size of zein-PG and zein-Pet / PG2:1 nanoparticles; Fig.11 This is the effect of NaCl on the potential of zein-PG and zein-Pet / PG2:1 nanoparticles.
[0071] The data show that with the increase of NaCl, the particle size of the nanoparticles gradually increases and the surface charge gradually decreases. When the NaCl concentration is greater than 10mM, the zein-PG nanoparticles aggregate and precipitate. For Zein-Pet / PG2:1 nanoparticles, when the concentration of NaCl solution increases from 0mM to 100mM, its ζ-potential significantly decreases from -24.47mV to -10.87mV, and the surface charge gradually decreases. When the NaCl concentration is greater than 50mM, the particle size of Z-Pet / PG2:1 nanoparticles increases significantly, and the nanoparticles slightly aggregate. This shows that the addition of NaCl solution reduces the electrostatic repulsion between nanoparticles through electrostatic shielding, neutralizes the charge on the surface of the nanoparticles, and thus causes particle aggregation. The addition of pectin reduces the aggregation of nanoparticles and increases the stability of nanoparticles in a salt ion environment.
[0072] (2) If Fig.12 As shown, Fig.12The figure shows the effect of ultraviolet light on the retention rate of prodigiosin in free prodigiosin, zein-PG, and zein-Pet / PG2:1 nanoparticles. Prodigiosin is easily affected by ultraviolet light and other light, and is easily degraded after ultraviolet irradiation. With the extension of ultraviolet irradiation time, the retention rate of prodigiosin gradually decreases. After ultraviolet irradiation, the retention rate of prodigiosin in zein-PG and zein-Pet / PG2:1 nanoparticles is higher than that of free prodigiosin, indicating that the encapsulation of zein and citrus pectin makes prodigiosin have better light stability and reduces its degradation. In addition, the retention rate of prodigiosin in zein-Pet / PG2:1 nanoparticles is higher than that in zein-PG nanoparticles, and the encapsulation of pectin forms a physical barrier to protect prodigiosin from ultraviolet irradiation.
[0073] The above description is only used to explain the preferred embodiment of the present invention, and it is determined that the optimal preparation condition is when the mass ratio of zein to citrus pectin in Example 1 is 2:1.
[0074] The present invention uses prodigiosin, zein and citrus pectin as raw materials, controls the mass ratio of zein to citrus pectin, and combines prodigiosin with zein and citrus pectin to prepare nanoparticles. The problem that prodigiosin is insoluble in water and easy to decompose is solved. The present invention uses bio-based materials as nanoparticle wall materials to ensure the safety of prodigiosin in practical applications. The present invention provides a method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles, which has the advantages of simple process, green safety, low cost, etc.
Claims
1. A zein-citrus pectin nanoparticle loaded with prodigiosin, Features: The structure of the nanoparticles is a core-shell structure with zein as the core and citrus pectin as the shell, prodigiosin enters the hydrophobic cavity of zein, and citrus pectin is wrapped on the surface of zein.
2. A method for preparing the prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 1, Features: The following steps are involved: S1, dissolving zein in 80% (V / V) ethanol aqueous solution to obtain a zein stock solution; S2, adding prodigiosin to the above zein stock solution, stirring with magnetic force at a speed of 600 rpm for 1 hour to fully dissolve the zein and prodigiosin, and adjusting the pH to 4.0 with 0.1 M HCl solution to obtain a zein-prodigiosin ethanol solution; S3, dissolving citrus pectin in ultrapure water to obtain a citrus pectin stock solution; S4, slowly adding the zein-prodigiosin ethanol solution obtained in S2 to ultrapure water with a pH of 4.0, mixing and stirring to obtain a dispersion of zein nanoparticles loaded with prodigiosin; The ethanol was removed by rotary evaporation under reduced pressure and heating, and then the dispersion was supplemented to the original volume with ultrapure water; S5, slowly dropwise adding the dispersion obtained in S4 into the citrus pectin solution, mixing and stirring evenly, with a stirring speed of 600 rpm for 1 hour, to obtain a dispersion of zein-citrus pectin nanoparticles loaded with prodigiosin, and storing at 4° C. away from light; S6. The dispersion of S5 was centrifuged at low speed to remove aggregates, and the supernatant was freeze-dried to obtain zein-citrus pectin nanoparticles loaded with prodigiosin.
3. The method for preparing the prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: In the step S1, the concentration of the zein stock solution is 5 g / L.
4. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: The mass ratio of zein to prodigiosin in the zein-prodigiosin ethanol solution is 10:
1.
5. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: The specific operation of step S3 is as follows: dissolve citrus pectin in ultrapure water, stir in a water bath at 65° C. and 600 rpm for 1 hour, cool to room temperature, and adjust the pH to 4.0 with 0.1 M NaOH solution to obtain a citrus pectin stock solution.
6. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 5, Features: The concentration of citrus pectin in step S3 is 2 g / L.
7. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: The conditions for the reduced pressure rotary evaporation in step S4 are as follows: a pressure of -0.1 MPa, a temperature of 45° C., and evaporation for 15 minutes.
8. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: In step S4, the volume ratio of the zein nanoparticle dispersion loaded with prodigiosin, zein-prodigiosin ethanol solution, to ultrapure water is 1:
4.
9. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: In step S5, the mass ratio of zein to citrus pectin is 20:1-1:
1.
10. The method for preparing prodigiosin-loaded zein-citrus pectin nanoparticles according to claim 2, Features: The centrifugal conditions in step S6 are: a rotation speed of 4000 rpm and a time of 10 min; the freeze-drying conditions are: a temperature of -45°C and a time of 72 h.
Citation Information
Patent Citations
Hyperin-loaded zein-pectin composite nanoparticles and preparation method thereof
CN112022834A
Preparation method of genipin cross-linked quercetin-zein / pectin / chitosan nanoparticles
CN114098076A
Preparation method of zein-premna microphylla pectin composite nanoparticles loaded with curcumin
CN116439364A
Method for coacervation of dihydroquercetin
RU2805649C1
Method to make hydrogels and cellulose from pectin- and protein-containing cellulosic biomass
US20240158584A1
Cited By
Lip care sunscreen microcapsule, preparation method and application of microcapsule in preparation of sunscreen activating lip balm
CN119818376A
Lip care sunscreen microcapsules and method of preparation and use in the preparation of a sunscreen and rejuvenating lip balm
CN119818376B