Preparation method of oxidation-resistant and high-temperature-resistant PPS filter material
By adding reaction tanks and rolls on the impregnation equipment and modifying the PPS filter material with special reaction liquid, the problem of easy oxidation of PPS filter material in high-temperature environment is solved, and the oxidation resistance and high-temperature resistance are improved and the amount of oxidation resistance and high-temperature resistance are achieved. Production capacity optimizes production efficiency and cost.
Patent Information
- Application Number
- CN202411234149.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-04
- Publication Date
- 2024-11-22
AI Technical Summary
PPS filters are susceptible to oxidation reactions in high temperature environments, which limits the expansion of their application fields. The existing modification methods are complex and have low mass production capabilities.
Add a reaction tank and a set of rolls to the original impregnation equipment, and use a special reaction liquid, including sodium hypochlorite solution, stabilizer and catalyst, to adjust the pH value and temperature, and modify the PPS filter material through the reaction liquid sex.
It has achieved the improvement of oxidation resistance and high temperature resistance of PPS filter materials, and supports mass production, which does not affect production capacity, controls production costs, and optimizes sample performance.
Smart Images

Figure CN118987784A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of PPS filter material modification, in particular to a method for preparing an oxidation-resistant and high-temperature-resistant PPS filter material. Background Art
[0002] PPS filter material is made of polyphenylene sulfide (PPS) fiber through opening, combing and other processes to form a composite product, and then after shaping, singeing and calendering, it can be formed after a post-treatment (coating / impregnation / laminating) if there are special needs. PPS filter material has good heat resistance, chemical resistance, flame retardancy and other characteristics. It can be used continuously in a working environment below 190°C. It is an ideal filter medium for bag dust removal and is widely used in dust collection and flue gas dust collection in coal-fired boilers, steel industry, chemical industry, etc. However, due to the low bond energy of PPS, it is susceptible to strong oxidizing gases in the environment under complex high-temperature environments and then undergoes oxidation reactions, resulting in the failure of the fiber material. When the O2 content in the treated flue gas exceeds 8% and the long-term operating temperature exceeds 160°C, the PPS filter material will also oxidize and fail, that is, the higher the O2 content in the environment, the lower the use temperature, which greatly limits the expansion of the application field of PPS filter material. Therefore, it is urgent to improve the oxidation resistance and temperature resistance of PPS filter material so that it can be used in a wider environment.
[0003] At present, there are many methods to modify PPS filter materials, but most of them start from raw materials such as PPS resin and PPS fiber, and the methods are cumbersome and complicated, and the mass production capacity is not high. Summary of the invention
[0004] The purpose of the present invention is to provide a method for preparing an oxidation-resistant and high-temperature-resistant PPS filter material, so as to solve the problems existing in the prior art and realize the mass production of the oxidation-resistant and high-temperature-resistant PPS filter material through simple equipment improvement.
[0005] In order to achieve the above object, the solution of the present invention is: A method for preparing an oxidation-resistant and high-temperature-resistant PPS filter material comprises a transmission shaft, a reaction tank, an immersion tank, an oven and a winding roller arranged in sequence along the forward direction of the PPS filter material, and two groups of rollers arranged between the reaction tank and the immersion tank, and between the immersion tank and the oven, and specifically comprises the following steps: Step 1. Adding an appropriate amount of stabilizer and catalyst to a sodium hypochlorite solution, and adjusting the pH value of the sodium hypochlorite solution to 7-9 with a weak acid solution to obtain a reaction solution, and adding the reaction solution to the reaction tank; Step 2. The PPS filter material is transported to the reaction tank by the transmission shaft, and is output by the first set of rollers after reacting with the reaction liquid, and then washed by the dipping tank and output by the second set of rollers, and then enters the oven for drying, and is rolled up by the winding roller after drying; The stabilizer is at least one of sodium silicate, sodium pyrophosphate, potassium hydrogen phthalate, sodium bicarbonate, sodium chloride, boron nitride, sodium bromide, disodium ethylenediaminetetraacetate, β-cyclodextrin, cellulose, aminosulfonic acid, phenanthroline, sodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium aminosulfonate, water-soluble oil, polyvinyl pyrrolidone, hydrochloric acid, disodium ethylenediaminetetraacetate (EDTA), potassium chloride, and stannous nitride; The catalyst is 2,2,6,6-tetramethylpiperidine-N-oxide or tetrapropylammonium perruthenate; The weak acid is at least one of carbonic acid, acetic acid, phosphoric acid, nitrous acid, hypochlorous acid, and dilute hydrochloric acid.
[0006] The mass of the stabilizer is 0.1-0.5 wt% of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; the mass of the catalyst is 0.1-0.5 wt% of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; and the concentration of the weak acid solution is 0.1-1 mol / L.
[0007] The available chlorine content of the sodium hypochlorite solution is 12-16%.
[0008] The reaction tank is a water bath.
[0009] The set temperature of the reaction tank is 30-35°C.
[0010] The water in the immersion tank is changed every 1.5 to 2 hours.
[0011] In step 2, the speed of the transmission shaft is set to 0.5-1 m / min, and the rolling allowances of the two sets of rollers are set to 110-120%.
[0012] In step 2, the oven is provided with 5 to 8 sections in total, and the temperature of the oven is set at 210 to 230°C.
[0013] After adopting the above technical solution, the present invention has the following technical effects: The present invention adds a reaction tank and a group of rollers to the original impregnation equipment, and adds a special reaction liquid into the reaction tank, so as to achieve mass production of PPS modified filter material while modifying the PPS filter material. For manufacturers, there is no need to add new production equipment lines, and accessories are added to the original automated production equipment, which does not affect the original production capacity and ensures the performance optimization of the sample, thereby achieving improved production efficiency and controlling production costs. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 It is a structural schematic diagram of a specific embodiment of the present invention; Description of Figure Numbers: 1- transmission shaft; 2- reaction tank; 3- immersion tank; 4- oven; 5- winding roller; 6- rolling roller; 10- PPS filter material. DETAILED DESCRIPTION
[0015] In order to further explain the technical solution of the present invention, the present invention is described in detail below through specific embodiments.
[0016] refer to Figure 1 As shown, the present invention discloses a method for preparing an oxidation-resistant and high-temperature-resistant PPS filter material, comprising a transmission shaft 1, a reaction tank 2, an immersion tank 3, an oven 4 and a winding roller 5 arranged in sequence along the forward direction of the PPS filter material 10, and two groups of rollers 6 arranged between the reaction tank 2 and the immersion tank 3, and between the immersion tank 3 and the oven 4, and specifically comprising the following steps: Step 1. Add an appropriate amount of stabilizer and catalyst to a sodium hypochlorite solution, and adjust the pH value of the sodium hypochlorite solution to 7-9 with a weak acid solution to obtain a reaction solution, and add the reaction solution to a reaction tank 2; Step 2. The PPS filter material 10 is transported to the reaction tank 2 by the transmission shaft 1, and is output by the first set of rollers 6 (left in the figure) after the reaction liquid reacts, and then is washed by the impregnation tank 3 and output by the second set of rollers 6 (right in the figure), and then enters the oven 4 for drying, and is rolled up by the winding roller 5 after drying, thereby completing the modification of the PPS filter material 10; The stabilizer is at least one of sodium silicate, sodium pyrophosphate, potassium hydrogen phthalate, sodium bicarbonate, sodium chloride, boron nitride, sodium bromide, disodium ethylenediaminetetraacetate, β-cyclodextrin, cellulose, aminosulfonic acid, phenanthroline, sodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium aminosulfonate, water-soluble oil, polyvinyl pyrrolidone, hydrochloric acid, disodium ethylenediaminetetraacetate (EDTA), potassium chloride, and stannous nitride; the catalyst is 2,2,6,6-tetramethylpiperidine-N-oxide (TEMPO) or tetrapropylammonium perruthenate (TPAP); the weak acid is at least one of carbonic acid, acetic acid, phosphoric acid, nitrous acid, hypochlorous acid, and dilute hydrochloric acid.
[0017] Through the above scheme, the present invention adds a reaction tank 2 and a group of rollers 6 to the original impregnation equipment, and adds a special reaction liquid into the reaction tank 2, so as to realize the mass production of PPS modified filter material while modifying the PPS filter material 10. For the manufacturer, there is no need to add new production equipment lines, and accessories are added to the original automated production equipment, which does not affect the original production capacity and ensures the performance optimization of the sample, thereby achieving improved production efficiency and controlling production costs.
[0018] Specific embodiments of the present invention are shown below.
[0019] The mass of the above-mentioned stabilizer is 0.1~0.5WT of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; the mass of the catalyst is 0.1~0.5WT of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; the concentration of the weak acid solution is 0.1~1mol / L.
[0020] The effective chlorine content of the above sodium hypochlorite solution is 12~16%.
[0021] The reaction tank 2 is a water bath or a device similar to a water bath, and a temperature control instrument and a power switch are provided on the panel thereof; the interior of the reaction tank 2 is provided with electric heating tubes and sensors, which can heat the reaction liquid and detect the temperature.
[0022] The set temperature of the reaction tank 2 is 30-35°C.
[0023] The above-mentioned immersion tank 3 is filled with sufficient clean water, and the clean water is replaced every 1.5 to 2 hours.
[0024] In the above step 2, the speed of the transmission shaft 1 is set to 0.5-1 m / min, and the rolling allowances of the two sets of rollers 6 are both set to 110-120%.
[0025] In the above step 2, the oven 4 is provided with 5 to 8 sections in total, and the temperature of the oven 4 is set to 210 to 230°C.
[0026] Several embodiments of the present invention are provided below. These embodiments are only preferred technical solutions of the present invention and are not intended to impose any limitation on the actual implementation of the present invention.
[0027] Example 1 is as follows: ①Prepare samples: PPS filter material sample, total length about 10m, width about 1m, surface density about 550g / m 2 ; ②Prepare the reaction solution: Pour 50kg of sodium hypochlorite solution (effective chlorine content: 13-16%) into reaction tank 2, add 50g of sodium silicate and 50g of tetrapropylammonium perruthenate; ③ Add 0.5 mol / L acetic acid to the above solution to adjust the pH value of the solution to about 9. The reaction solution has been prepared; ④ Adjust the reaction tank temperature to 35°C; ⑤ The PPS filter material 10 passes through the transmission roller 1 at a speed of 0.5m / min, reaches the reaction tank 2 which has reached the set temperature of 35°C, reacts with the reaction liquid, and is controlled to have a rolling residue of 110% by the roller 6 at the outlet of the reaction tank 2, reaches the immersion tank 3 for water washing, and then controls the rolling residue of 115% by the roller 6 at the outlet of the immersion tank 3, enters the 7-section drying oven 4 which has reached the set temperature of 220°C, and is finally rolled by the transmission roller 5 to obtain an oxidation-resistant and high-temperature resistant PPS filter material.
[0028] Example 2 is as follows: The difference from Example 1 is that the speed of the driving roller 1 is set to 1.0 m / min.
[0029] Example 3 is as follows: The difference from Example 1 is that the speed of the driving roller 1 is set to 1.5 m / min.
[0030] Embodiment 4 is as follows: The difference from Example 1 is that the temperature of the reaction tank 2 is set to 30°C.
[0031] Example 5 is as follows: The difference from Example 1 is that the temperature of the reaction tank 2 is set to 40°C.
[0032] The nitric acid resistance and temperature resistance of the PPS modified filter material and the unmodified PPS filter material obtained in Examples 1-5 were tested under the following test conditions: a. Nitric acid resistance The filter material was immersed in a 15% HNO3 solution and left to stand at 93°C for 24 hours before testing its tensile strength and comparing it with the untreated PPS filter material. b. Heat resistance The filter material was placed in an oven at 280°C, and its tensile strength was tested after 24 hours, and compared with that of untreated PPS filter material.
[0033] The test results are as follows:
[0034] It can be seen from the above table: The unmodified PPS filter material has a breaking strength retention rate of 56% to 61% after the oxidation resistance test (nitric acid soaking), and a breaking strength retention rate of 49% to 55% after the high temperature resistance test (280°C); the breaking strength retention rate of the samples of Example 1, Example 2 and Example 4 after the oxidation resistance test is 81% to 89%, and the breaking strength retention rate after the high temperature resistance test is 69% to 78%. This shows that the oxidation resistance and high temperature resistance of the modified PPS filter material are improved.
[0035] The above embodiments and drawings do not limit the product form and style of the present invention. Any appropriate changes or modifications made by ordinary technicians in the relevant technical field should be deemed to be within the patent scope of the present invention.
Claims
1. A method for preparing an oxidation-resistant and high-temperature-resistant PPS filter material, characterized in that The invention comprises a transmission shaft, a reaction tank, an immersion tank, an oven and a winding roller which are sequentially arranged along the forward direction of the PPS filter material, and two groups of rollers which are arranged between the reaction tank and the immersion tank and between the immersion tank and the oven, and specifically comprises the following steps: Step 1. Adding an appropriate amount of stabilizer and catalyst to a sodium hypochlorite solution, and adjusting the pH value of the sodium hypochlorite solution to 7-9 with a weak acid solution to obtain a reaction solution, and adding the reaction solution to the reaction tank; Step 2. The PPS filter material is transported to the reaction tank by the transmission shaft, and is output by the first set of rollers after reacting with the reaction liquid, and then washed by the dipping tank and output by the second set of rollers, and then enters the oven for drying, and is rolled up by the winding roller after drying; The stabilizer is at least one of sodium silicate, sodium pyrophosphate, potassium hydrogen phthalate, sodium bicarbonate, sodium chloride, boron nitride, sodium bromide, disodium ethylenediaminetetraacetate, β-cyclodextrin, cellulose, aminosulfonic acid, phenanthroline, sodium phosphate, disodium hydrogen phosphate, sodium dihydrogen phosphate, sodium aminosulfonate, water-soluble oil, polyvinyl pyrrolidone, hydrochloric acid, disodium ethylenediaminetetraacetate (EDTA), potassium chloride, and stannous nitride; The catalyst is 2,2,6,6-tetramethylpiperidine-N-oxide or tetrapropylammonium perruthenate; The weak acid is at least one of carbonic acid, acetic acid, phosphoric acid, nitrous acid, hypochlorous acid, and dilute hydrochloric acid.
2. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: The mass of the stabilizer is 0.1-0.5 wt% of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; the mass of the catalyst is 0.1-0.5 wt% of the total mass of the sodium hypochlorite solution, the stabilizer and the catalyst; and the concentration of the weak acid solution is 0.1-1 mol / L.
3. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: The available chlorine content of the sodium hypochlorite solution is 12-16%.
4. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: The reaction tank is a water bath.
5. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: The set temperature of the reaction tank is 30-35°C.
6. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: The water in the immersion tank is changed every 1.5 to 2 hours.
7. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: In step 2, the speed of the transmission shaft is set to 0.5-1 m / min, and the rolling allowances of the two sets of rollers are set to 110-120%.
8. The method for preparing the oxidation-resistant and high-temperature-resistant PPS filter material according to claim 1, characterized in that: In step 2, the oven is provided with 5 to 8 sections in total, and the temperature of the oven is set at 210 to 230°C.
Citation Information
Patent Citations
Stabilizing agent for sodium hypochlorite and usage method thereof
CN105961382A
Denitration and dust removal integrated filter material preparation method and prepared filter material
CN112704959A
Method for simply and conveniently preparing high-temperature-resistant antioxidant polyphenylene sulfide fiber and product of high-temperature-resistant antioxidant polyphenylene sulfide fiber
CN116556046A