High-temperature-resistant filtering material as well as preparation method and application thereof

By preparing a high-temperature resistant filter material combining a V2O5-CeO2-TiO2/activated carbon multi-component catalyst with a polytetrafluoroethylene microporous membrane, the problems of low dioxin removal efficiency and high cost in the existing technology were solved, and a highly efficient and high-temperature resistant dioxin degradation effect was achieved.

CN118987793AActive Publication Date: 2024-11-22WUHAN TEXTILE UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411394149.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-08
Publication Date
2024-11-22
Estimated Expiration
2044-10-08

AI Technical Summary

Technical Problem

Existing technologies are insufficient for the efficient removal of dioxins, and precious metal catalysts are costly and inefficient, while activated carbon adsorption and regeneration are inefficient and prone to causing secondary pollution.

Method used

A high-temperature resistant filter material was prepared by mixing tetrabutyl titanate, acetic acid, and activated carbon, and adding ammonium metavanadate and cerium nitrate hexahydrate to form a V2O5-CeO2-TiO2/activated carbon multi-component composite catalyst. After acidification treatment, the catalyst was combined with a polytetrafluoroethylene microporous membrane to form a high-temperature resistant filter material.

Benefits of technology

It effectively removes dioxins at high temperatures, improves adsorption capacity and catalytic activity, has high degradation efficiency, and strong resistance to alkali metal poisoning, making it suitable for coal-fired power plants, thermal power generation and other fields.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118987793A_ABST
    Figure CN118987793A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of filtering materials, and provides a high-temperature-resistant filtering material as well as a preparation method and application thereof. The method comprises the following steps: adding TiO2 / activated carbon powder into ammonium metavanadate, cerium nitrate hexahydrate and water, calcining, and acidizing to obtain an acidized composite catalyst; spinning the organic matter and the acidified composite catalyst, and then carrying out pre-needling and main needling; the needled felt is soaked in the catalyst suspension and then dried, the upper surface and the lower surface of the dried needled felt are coated with polytetrafluoroethylene foam coating in a blade coating mode, and then a polytetrafluoroethylene microporous membrane is hot-pressed on the upper surface. By adding the activated carbon subjected to high-temperature heat treatment, the adsorption capacity of the activated carbon to dioxin is increased, and meanwhile, the activated carbon and the composite catalyst have a synergistic effect, so that the removal rate of the dioxin is increased while the dust removal and filtration efficiency is ensured. The composite catalyst is acidized, so that active components in the filter material are protected, and the catalytic activity and the alkali metal poisoning resistance of the filter material are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of filter materials, and in particular to a high temperature resistant filter material and a preparation method and application thereof. Background Art

[0002] Dioxin is a general term for chlorinated polynuclear aromatic compounds, including polychlorinated bibenzo dioxins (PCDDs) and polychlorinated bibenzo furans (PCDFs). Dioxin is a pollutant that can cause serious harm to organisms. It can exist in the environment for a long time. Once it enters an organism, it will accumulate in the organism and is difficult to be excreted. With the continuous acceleration of the industrialization process, environmental pollution problems caused by high-temperature exhaust gas emissions and waste burning are becoming more and more serious. Dioxins are mainly produced during the incineration of waste and can enter the surrounding environment through flue gas, fly ash, etc., causing serious air pollution and threatening national health.

[0003] In the early stage, dioxins were mainly removed by adsorbing them on the surface and in the pores of activated carbon. For example, Chinese patent CN118320794A discloses that dioxins can be adsorbed by activated carbon, but this method cannot degrade dioxins, and the regeneration efficiency is low, and secondary pollution is easily caused during the regeneration process. At present, dioxins are mainly eliminated by catalytic degradation of precious metals and transition metal catalysts. Dioxin catalytic technology can degrade dioxins to generate carbon dioxide, hydrogen chloride and water through redox reactions. It has the characteristics of low energy consumption, high efficiency and few secondary pollutants, and can directly decompose harmful substances into harmless substances. For example, Chinese patent CN115845873A provides a catalyst composed of precious metal Pt and transition metal Ni that can degrade dioxins at low temperatures, but the cost is high and the degradation efficiency is low.

[0004] Therefore, it is of great significance to propose a high-temperature resistant filter material that can efficiently eliminate harmful gases based on catalytic degradation technology. Summary of the invention

[0005] The purpose of the present invention is to provide a high temperature resistant filter material and a preparation method and application thereof in order to overcome the deficiencies of the prior art.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a method for preparing a high temperature resistant filter material, comprising the following steps:

[0008] 1) mixing tetrabutyl titanate, acetic acid, anhydrous ethanol and activated carbon to obtain a slurry; calcining the slurry to obtain TiO2 / activated carbon powder;

[0009] 2) mixing ammonium metavanadate, cerium nitrate hexahydrate and water to obtain a mixed solution; adding TiO2 / activated carbon powder to the mixed solution to obtain a mud material; calcining the mud material to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst;

[0010] 3) acidifying, washing and drying the multi-component composite catalyst in sequence to obtain an acidified composite catalyst;

[0011] 4) spinning the organic matter and the acidified composite catalyst, and then performing pre-needling and main needling in sequence to obtain a needle-punched felt;

[0012] 5) subjecting the acidified composite catalyst and water to ultrasonic vibration to obtain a catalyst suspension; immersing the needle-punched felt in the catalyst suspension and drying it to obtain a catalyst-loaded needle-punched felt;

[0013] 6) mixing the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water and foaming them to obtain a foam coating;

[0014] 7) The foam coating is scraped onto the upper and lower surfaces of the catalyst-loaded needle-punched felt, and then a polytetrafluoroethylene microporous membrane is hot-pressed onto the upper surface of the needle-punched felt to obtain a high-temperature resistant filter material.

[0015] Preferably, in step 1), the volume ratio of tetrabutyl titanate, acetic acid and anhydrous ethanol is 1:1.2-2:4.4-5.5, and the volume ratio of the total volume of tetrabutyl titanate, acetic acid and anhydrous ethanol to the volume ratio of activated carbon is 1:0.8-1.2;

[0016] The calcination temperature is 900-950° C., the calcination time is 2-4 hours, and the calcination atmosphere is a nitrogen atmosphere.

[0017] Preferably, in step 2), the mass ratio of ammonium metavanadate to cerium nitrate hexahydrate is 1:0.6-0.8, and the mass concentration of the mixed solution is 2-10%;

[0018] The mixing temperature is 60-80° C., the mixing time is 3-4 hours, the calcining temperature is 400-500° C., the calcining time is 2-4 hours, and the calcining atmosphere is a nitrogen atmosphere.

[0019] Preferably, the reagent for the acidification treatment in step 3) is sulfuric acid, the concentration of the sulfuric acid is 0.08-0.12 mol / L, the acidification treatment time is 4-6 hours, the washing reagent is water, and the washing is performed until the pH value of the multi-component composite catalyst no longer changes; the drying temperature is 90-105° C., and the drying time is 12-18 hours.

[0020] Preferably, in step 4), the mass ratio of the organic matter to the acidified composite catalyst is 10-30:70-90, and the organic matter comprises one or more of polyetheretherketone, polytetrafluoroethylene and polyphenylene sulfide;

[0021] The depth of the pre-needling is 10-14 mm, and the density is 70-140 needles / cm 2 The main acupuncture depth is 6-12 mm, and the density is 1000-1500 needles / cm 2 .

[0022] Preferably, in step 5), the mass concentration of the catalyst suspension is 1-8%, the immersion time is 6-8 hours, and the drying temperature is 80-100° C.

[0023] The catalyst loading of the needle felt is 80 to 120 g / m 2 ; The total weight of needle felt is 200~600g / m 2 .

[0024] Preferably, in step 6), the solid content of the polytetrafluoroethylene dispersion is 57-63%; the mass ratio of the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water is 1.5-2: 0.05-0.1: 0.6-1: 97-98;

[0025] The foaming time is 10 to 15 minutes, and stirring is performed during the foaming process at a stirring rate of 3000 to 5000 r / min; the foaming ratio of the foam coating is 4 to 6:1;

[0026] The foaming agent is sodium cocoylamphoacetate or alkyl glucoside, and the stabilizer is Tween 80 or sodium lauryl sulfate.

[0027] Preferably, the thickness of the scraping in step 7) is 0.4-0.6 cm; the temperature of the hot pressing is 200-300° C., the time of the hot pressing is 8-10 s, and the pressure of the hot pressing is 1-3 MPa;

[0028] The weight of the polytetrafluoroethylene microporous membrane is 3 to 4 g / m 2 , thickness is 10-15μm, pore size is 0.6-0.8μm, air permeability is 70-100L / m 2 ·s.

[0029] The invention also provides a high temperature resistant filter material prepared by the preparation method.

[0030] The invention also provides application of the high temperature resistant filter material in removing dioxins.

[0031] The beneficial effects of the present invention include the following:

[0032] 1) The high temperature resistant filter material of the present invention reduces the content of oxygen-containing functional groups on the surface of the activated carbon by adding high temperature heat treatment, increases the adsorption capacity of the activated carbon for dioxins, and synergizes with the composite catalyst to improve the removal rate of dioxins by the material while ensuring the dust removal and filtration efficiency.

[0033] 2) The present invention protects the active components in the filter material by subjecting the composite catalyst to acid treatment, thereby improving its catalytic activity and ability to resist alkali metal poisoning.

[0034] 3) The filter material of the present invention can be used for a long time at a temperature of 230-260°C, and the instantaneous maximum use temperature can even reach 280°C. The high temperature resistant filter material of the present invention can be prepared into filter bags or filter cartridges, and used as a dust removal device in multiple fields such as coal burning, thermal power generation, asphalt, steel, and garbage incineration. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 The present invention is a flow chart of the preparation process of the high temperature resistant filter material. DETAILED DESCRIPTION

[0036] The present invention provides a method for preparing a high temperature resistant filter material, comprising the following steps:

[0037] 1) mixing tetrabutyl titanate, acetic acid, anhydrous ethanol and activated carbon to obtain a slurry; calcining the slurry to obtain TiO2 / activated carbon powder;

[0038] 2) mixing ammonium metavanadate, cerium nitrate hexahydrate and water to obtain a mixed solution; adding TiO2 / activated carbon powder to the mixed solution to obtain a mud material; calcining the mud material to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst;

[0039] 3) acidifying, washing and drying the multi-component composite catalyst in sequence to obtain an acidified composite catalyst;

[0040] 4) spinning the organic matter and the acidified composite catalyst, and then performing pre-needling and main needling in sequence to obtain a needle-punched felt;

[0041] 5) subjecting the acidified composite catalyst and water to ultrasonic vibration to obtain a catalyst suspension; immersing the needle-punched felt in the catalyst suspension and drying it to obtain a catalyst-loaded needle-punched felt;

[0042] 6) mixing the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water and foaming them to obtain a foam coating;

[0043] 7) The foam coating is scraped onto the upper and lower surfaces of the catalyst-loaded needle-punched felt, and then a polytetrafluoroethylene microporous membrane is hot-pressed onto the upper surface of the needle-punched felt to obtain a high-temperature resistant filter material.

[0044] In the present invention, the volume ratio of tetrabutyl titanate, acetic acid and anhydrous ethanol in step 1) is preferably 1:1.2-2:4.4-5.5, more preferably 1:1.4-1.8:4.6-5.2, and more preferably 1:1.6:4.8-5.0; the volume ratio of the total volume of tetrabutyl titanate, acetic acid and anhydrous ethanol to the volume ratio of activated carbon is preferably 1:0.8-1.2, more preferably 1:0.9-1.1, and more preferably 1:1;

[0045] The calcination temperature is preferably 900-950°C, more preferably 910-940°C, more preferably 920-930°C, the calcination time is preferably 2-4h, more preferably 2.5-3.5h, more preferably 3h, and the calcination atmosphere is preferably a nitrogen atmosphere.

[0046] In the present invention, the concentration of acetic acid is preferably 0.8 to 1 mol / L, more preferably 0.9 mol / L.

[0047] In the present invention, the mixing in step 1) is preferably a first mixing of tetrabutyl titanate, acetic acid and anhydrous ethanol, and a second mixing of the first mixed solution and activated carbon; the time for the first mixing is preferably 15 to 25 minutes, more preferably 18 to 22 minutes, and more preferably 20 minutes, and magnetic stirring is performed during the first mixing.

[0048] In the present invention, after the calcination in step 1) is completed, the calcined product is preferably crushed and sieved to obtain TiO2 / activated carbon powder; the mesh size of the sieve is preferably 60 mesh.

[0049] In the present invention, the mass ratio of the ammonium metavanadate and the cerium nitrate hexahydrate in step 2) is preferably 1:0.6-0.8, more preferably 1:0.65-0.75, more preferably 1:0.7, and the mass concentration of the mixed solution is preferably 2-10%, more preferably 3-8%, and more preferably 5-6%.

[0050] In the present invention, the mass ratio of TiO2 / activated carbon powder to mixed solution is preferably 0.6 to 0.8:1, more preferably 0.65 to 0.75:1, and more preferably 0.7:1.

[0051] In the present invention, the mixing temperature in step 2) is preferably 60-80°C, more preferably 65-75°C, more preferably 70°C, the mixing time is preferably 3-4h, more preferably 3.5h, the calcination temperature is preferably 400-500°C, more preferably 420-480°C, more preferably 440-450°C, the calcination time is preferably 2-4h, more preferably 2.5-3.5h, more preferably 3h, and the calcination atmosphere is preferably a nitrogen atmosphere.

[0052] In the present invention, after the calcination in step 2) is completed, the calcined product is preferably crushed and sieved to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst; the mesh size of the sieve is preferably 60 meshes.

[0053] In the present invention, the reagent for the acidification treatment in step 3) is preferably sulfuric acid, the concentration of sulfuric acid is preferably 0.08-0.12 mol / L, more preferably 0.09-0.11 mol / L, more preferably 0.1 mol / L, the time for the acidification treatment is preferably 4-6 h, more preferably 4.5-5.5 h, more preferably 5 h; the washing reagent is preferably water, and the pH value of the multi-component composite catalyst no longer changes after washing; the drying temperature is preferably 90-105 ° C, more preferably 95-100 ° C, and the drying time is preferably 12-18 h, more preferably 13-17 h, more preferably 15-16 h.

[0054] In the present invention, the mass ratio of the organic matter and the acidified composite catalyst in step 4) is preferably 10-30:70-90, more preferably 15-25:75-85, and more preferably 20:80; the organic matter preferably comprises one or more of polyetheretherketone, polytetrafluoroethylene and polyphenylene sulfide.

[0055] In the present invention, the specific spinning process is preferably: placing the acidified composite catalyst in anhydrous ethanol and ultrasonically oscillating at 100 Hz for 2 hours to obtain a dispersion with a mass concentration of 10-20%, grinding the organic granules into powder form, adding the organic powder to the dispersion (the mass ratio of the organic powder to the acidified composite catalyst is 10-30:70-90), and stirring in a mechanical mixer rotating at 200r / min for 24 hours until the mixture is half dry. The mixture is dried in an oven at 60°C for 48 hours, and melt-spinned after removing the solvent. The spinning temperature is 415°C, the hot tunnel temperature is 300°C, the drafting multiple is 3 times, the drafting temperature is 200°C, the drafting rate is 200cm / min, and the linear density of the fiber obtained by spinning is 21.13dtex, the breaking strength can reach 3.94cN / dtex, and the breaking elongation is 14.73%.

[0056] In the present invention, the depth of the pre-needling in step 4) is preferably 10 to 14 mm, more preferably 11 to 13 mm, and more preferably 12 mm, and the density is preferably 70 to 140 needles / cm 2 , more preferably 80 to 120 needles / cm 2 , more preferably 100 to 110 needles / cm 2 The main acupuncture depth is preferably 6 to 12 mm, more preferably 8 to 10 mm, more preferably 9 mm, and the density is preferably 1000 to 1500 needles / cm 2, more preferably 1100 to 1400 needles / cm 2 , more preferably 1200 to 1300 needles / cm 2 .

[0057] In the present invention, the mass concentration of the catalyst suspension in step 5) is preferably 1-8%, more preferably 3-6%, and more preferably 4-5%; the immersion time is preferably 6-8h, more preferably 6.5-7.5h, and more preferably 7h; the drying temperature is preferably 80-100°C, more preferably 85-95°C, and more preferably 90°C;

[0058] The catalyst loading of the needle felt is preferably 80 to 120 g / m 2 , more preferably 90 to 110 g / m 2 The total weight of the needle felt is preferably 200 to 600 g / m 2 , more preferably 300 to 500 g / m 2 .

[0059] In the present invention, the solid content of the polytetrafluoroethylene dispersion in step 6) is preferably 57-63%, more preferably 58-62%, and more preferably 60-61%; the mass ratio of the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water is preferably 1.5-2: 0.05-0.1: 0.6-1: 97-98, more preferably 1.6-1.9: 0.06-0.09: 0.7-0.9: 97.2-97.8, and more preferably 1.7-1.8: 0.07-0.08: 0.8: 97.5-97.6.

[0060] In the present invention, the foaming time in step 6) is preferably 10 to 15 minutes, more preferably 11 to 14 minutes, and more preferably 12 to 13 minutes; stirring is performed during the foaming process, and the stirring rate is preferably 3000 to 5000 r / min, more preferably 3500 to 4500 r / min, and more preferably 4000 r / min; the foaming ratio of the foam coating is preferably 4 to 6:1, more preferably 4.5 to 5.5:1, and more preferably 5:1;

[0061] The foaming agent is preferably sodium cocoyl amphoacetate or alkyl glucoside, and the stabilizer is preferably Tween 80 or sodium lauryl sulfate.

[0062] In the present invention, the polytetrafluoroethylene foam coating not only fixes the catalyst particles on the needle-punched felt, but also increases the bonding strength between the needle-punched felt and the PTFE microporous membrane.

[0063] In the present invention, the thickness of the scraping in step 7) is preferably 0.4 to 0.6 cm, more preferably 0.45 to 0.55 cm, and more preferably 0.5 cm; the temperature of the hot pressing is preferably 200 to 300°C, more preferably 220 to 280°C, and more preferably 240 to 250°C; the time of the hot pressing is preferably 8 to 10 s, and more preferably 9 s; the pressure of the hot pressing is preferably 1 to 3 MPa, more preferably 1.5 to 2.5 MPa, and more preferably 2 MPa.

[0064] In the present invention, the weight of the polytetrafluoroethylene microporous membrane in step 7) is preferably 3 to 4 g / m 2 , more preferably 3.5g / m 2 The thickness is preferably 10 to 15 μm, more preferably 11 to 14 μm, more preferably 12 to 13 μm, the pore size is preferably 0.6 to 0.8 μm, more preferably 0.7 μm, and the air permeability is preferably 70 to 100 L / m 2 ·s, more preferably 80 to 90 L / m 2 ·s.

[0065] In the present invention, the polytetrafluoroethylene (PTFE) microporous membrane mainly plays a dust removal role in the filter material, so that the filtration efficiency of the filter material is not less than 99.75%; the present invention uses one or more of polyetheretherketone, polytetrafluoroethylene and polyphenylene sulfide fibers and a catalyst for mixed spinning, and obtains a needle-punched felt through mixed opening, carding, web laying, needle punching, trimming and winding, and uses the needle-punched felt as the matrix of the composite catalytic filter bag.

[0066] The invention also provides a high temperature resistant filter material prepared by the preparation method.

[0067] The invention also provides application of the high temperature resistant filter material in removing dioxins.

[0068] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0069] In the embodiment, the specific process of mixed spinning of polyetheretherketone and acidified composite catalyst is as follows: placing the acidified composite catalyst in anhydrous ethanol and ultrasonically oscillating at 100Hz for 2h to obtain a dispersion with a mass concentration of 15%, grinding the polyetheretherketone pellets into powder form, adding the polyetheretherketone powder to the dispersion (the mass ratio of the polyetheretherketone powder to the acidified composite catalyst is 20:80), and stirring in a mechanical mixer rotating at 200r / min for 24h until the mixture is half dry. The mixture is dried in an oven at 60°C for 48h, and melt-spun after removing the solvent. The spinning temperature is 415°C, the hot tunnel temperature is 300°C, the draft multiple is 3 times, the draft temperature is 200°C, the draft rate is 200cm / min, and the linear density of the fiber obtained by spinning is 21.13dtex, the breaking strength can reach 3.94cN / dtex, and the breaking elongation is 14.73%.

[0070] Example 1

[0071] Tetrabutyl titanate, acetic acid (concentration of 0.8 mol / L) and anhydrous ethanol in a volume ratio of 1:1.2:4.4 were mixed, and magnetic stirring (speed of 500 r / min) was performed for 20 min to obtain a mixed solution; the mixed solution was evenly mixed with activated carbon in a volume ratio of 1:0.8 to obtain a mud material, and the mud material was calcined at 950°C for 4 h under a nitrogen atmosphere. The calcined product was crushed and passed through a 60-mesh sieve to obtain TiO2 / activated carbon powder.

[0072] Ammonium metavanadate and cerium nitrate hexahydrate in a mass ratio of 1:0.6 are added to deionized water at 60°C, and stirred for 4 hours to obtain a mixed solution with a mass concentration of 6%; TiO2 / activated carbon powder is added to the mixed solution (the mass ratio of TiO2 / activated carbon powder and mixed solution is 0.6:1) and mixed evenly to obtain mud, which is calcined at 400°C for 2 hours under a nitrogen atmosphere, and the calcined product is crushed and passed through a 60-mesh sieve to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst.

[0073] The multi-component composite catalyst was acidified by soaking it in 0.1 mol / L sulfuric acid for 4 hours, and then the composite catalyst was washed with deionized water until the pH value no longer changed. The composite catalyst was then dried in an oven at 90° C. for 12 hours to obtain an acidified composite catalyst.

[0074] The polyetheretherketone and the acidified composite catalyst are mixed and spun, and the fiber filaments are mixed, opened, combed, laid, needled, trimmed and wound to obtain a needle-punched felt. After the fiber filaments are laid, they are pre-needled to form a preliminary embryo felt. The pre-needling depth is 10 mm and the pre-needling density is 80 needles / cm 2 After the pre-needling, the upper and lower needle-punching machines are used for the main needling to reinforce the needle-punched felt. The main needling depth is 6mm and the main needling density is 1100 needles / cm2 ; Needle felt is used as the base of composite catalytic filter bag, with a total weight of 350g / m 2 .

[0075] The prepared acidified composite catalyst was placed in deionized water and subjected to ultrasonic oscillation (frequency of 100 Hz) for 2 h to obtain a catalyst suspension with a mass concentration of 2%. The needle felt was immersed in the catalyst suspension for 6 h and then dried at 80 ° C to obtain a catalyst-loaded needle felt. The catalyst loading of the needle felt was 85 g / m 2 .

[0076] A PTFE concentrated dispersion (the solid content of the PTFE concentrated dispersion is 60%), a stabilizer, sodium dodecyl sulfate, a foaming agent, an alkyl polyglycoside (APG), and deionized water are mixed (the mass ratio of the PTFE concentrated dispersion, the stabilizer, the foaming agent, and the deionized water is 1.5:0.05:0.6:97), and the mixed solution is foamed in a stirrer, and the stirrer stirs at a high speed of 3500r / min for 10 minutes to obtain a stable foam coating with a foaming ratio of 4:1; the foam coating is scraped on the upper and lower surfaces of the catalyst-loaded needle felt by a scraper (the thickness of the upper and lower surfaces is 0.5cm), and then a layer of PTFE microporous membrane is hot-pressed on the upper surface, and the gram weight of the PTFE microporous membrane is 3g / m 2 , thickness is 12μm, pore size is 0.6μm, air permeability is 80L / m 2 ·s; the hot pressing temperature is 250°C, the time is 9s, and the pressure is 2MPa to obtain a high temperature resistant filter material.

[0077] Example 2

[0078] Tetrabutyl titanate, acetic acid (concentration of 0.9 mol / L) and anhydrous ethanol in a volume ratio of 1:1.6:4.8 were mixed, and magnetic stirring (speed of 500 r / min) was performed for 20 min to obtain a mixed solution; the mixed solution was evenly mixed with activated carbon in a volume ratio of 1:0.8 to obtain a mud material, and the mud material was calcined at 950°C for 4 h under a nitrogen atmosphere. The calcined product was crushed and passed through a 60-mesh sieve to obtain TiO2 / activated carbon powder.

[0079] Ammonium metavanadate and cerium nitrate hexahydrate in a mass ratio of 1:0.6 are added to deionized water at 60°C, and stirred for 4 hours to obtain a mixed solution with a mass concentration of 6%; TiO2 / activated carbon powder is added to the mixed solution (the mass ratio of TiO2 / activated carbon powder and mixed solution is 0.6:1) and mixed evenly to obtain mud, which is calcined at 400°C for 2 hours under a nitrogen atmosphere, and the calcined product is crushed and passed through a 60-mesh sieve to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst.

[0080] The multi-component composite catalyst was soaked in 0.1 mol / L sulfuric acid for 4 hours for acidification treatment, and then the composite catalyst was washed with deionized water until the pH value no longer changed. Then, the composite catalyst was dried in an oven at 100° C. for 12 hours to obtain an acidified composite catalyst.

[0081] The polyetheretherketone and the acidified composite catalyst are mixed and spun, and the fiber filaments are mixed, opened, combed, laid, needled, trimmed and wound to obtain a needle-punched felt. After the fiber filaments are laid, they are pre-needled to form a preliminary embryo felt. The pre-needling depth is 10 mm and the pre-needling density is 80 needles / cm 2 After the pre-needling, the upper and lower needle-punching machines are used for the main needling to reinforce the needle-punched felt. The main needling depth is 6mm and the main needling density is 1100 needles / cm 2 ; Needle felt is used as the base of composite catalytic filter bag, with a total weight of 350g / m 2 .

[0082] The prepared acidified composite catalyst was placed in deionized water and subjected to ultrasonic oscillation (frequency of 100 Hz) for 2 h to obtain a catalyst suspension with a mass concentration of 2%. The needle felt was immersed in the catalyst suspension for 6 h and then dried at 80 ° C to obtain a catalyst-loaded needle felt. The catalyst loading of the needle felt was 85 g / m 2 .

[0083] A PTFE concentrated dispersion (the solid content of the PTFE concentrated dispersion is 60%), a stabilizer, sodium dodecyl sulfate, a foaming agent, an alkyl polyglycoside (APG), and deionized water are mixed (the mass ratio of the PTFE concentrated dispersion, the stabilizer, the foaming agent, and the deionized water is 1.5:0.05:0.6:97), and the mixed solution is foamed in a stirrer, and the stirrer stirs at a high speed of 3500r / min for 10 minutes to obtain a stable foam coating with a foaming ratio of 4:1; the foam coating is scraped on the upper and lower surfaces of the catalyst-loaded needle felt by a scraper (the thickness of the upper and lower surfaces is 0.5cm), and then a layer of PTFE microporous membrane is hot-pressed on the upper surface, and the gram weight of the PTFE microporous membrane is 3g / m 2 , thickness is 12μm, pore size is 0.6μm, air permeability is 80L / m 2 ·s; the hot pressing temperature is 250°C, the time is 9s, and the pressure is 2MPa to obtain a high temperature resistant filter material.

[0084] Example 3

[0085] Tetrabutyl titanate, acetic acid (concentration of 1 mol / L) and anhydrous ethanol in a volume ratio of 1:1.2:4.4 were mixed, and magnetic stirring (speed of 500 r / min) was performed for 20 min to obtain a mixed solution; the mixed solution was evenly mixed with activated carbon in a volume ratio of 1:0.8 to obtain a mud material, and the mud material was calcined at 950°C for 4 h under a nitrogen atmosphere. The calcined product was crushed and passed through a 60-mesh sieve to obtain TiO2 / activated carbon powder.

[0086] Ammonium metavanadate and cerium nitrate hexahydrate in a mass ratio of 1:0.7 are added to deionized water at 70°C, and stirred for 4 hours to obtain a mixed solution with a mass concentration of 8%; TiO2 / activated carbon powder is added to the mixed solution (the mass ratio of TiO2 / activated carbon powder and mixed solution is 0.6:1) and mixed evenly to obtain mud, which is calcined at 450°C for 2 hours under a nitrogen atmosphere, and the calcined product is crushed and passed through a 60-mesh sieve to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst.

[0087] The multi-component composite catalyst was acidified by soaking it in 0.1 mol / L sulfuric acid for 4 hours, and then the composite catalyst was washed with deionized water until the pH value no longer changed. The composite catalyst was then dried in an oven at 90° C. for 12 hours to obtain an acidified composite catalyst.

[0088] The polyetheretherketone and the acidified composite catalyst are mixed and spun, and the fiber filaments are mixed, opened, combed, laid, needled, trimmed and wound to obtain a needle-punched felt. After the fiber filaments are laid, they are pre-needled to form a preliminary embryo felt. The pre-needling depth is 10 mm and the pre-needling density is 80 needles / cm 2 After the pre-needling, the upper and lower needle-punching machines are used for the main needling to reinforce the needle-punched felt. The main needling depth is 6mm and the main needling density is 1100 needles / cm 2 ; Needle felt is used as the base of composite catalytic filter bag, with a total weight of 350g / m 2 .

[0089] The prepared acidified composite catalyst was placed in deionized water and subjected to ultrasonic oscillation (frequency of 100 Hz) for 2 h to obtain a catalyst suspension with a mass concentration of 2%. The needle felt was immersed in the catalyst suspension for 6 h and then dried at 80 ° C to obtain a catalyst-loaded needle felt. The catalyst loading of the needle felt was 85 g / m 2 .

[0090] A PTFE concentrated dispersion (the solid content of the PTFE concentrated dispersion is 60%), a stabilizer, sodium dodecyl sulfate, a foaming agent, an alkyl polyglycoside (APG), and deionized water are mixed (the mass ratio of the PTFE concentrated dispersion, the stabilizer, the foaming agent, and the deionized water is 1.5:0.05:0.6:97), and the mixed solution is foamed in a stirrer, and the stirrer stirs at a high speed of 3500r / min for 10 minutes to obtain a stable foam coating with a foaming ratio of 4:1; the foam coating is scraped on the upper and lower surfaces of the catalyst-loaded needle felt by a scraper (the thickness of the upper and lower surfaces is 0.5cm), and then a layer of PTFE microporous membrane is hot-pressed on the upper surface, and the gram weight of the PTFE microporous membrane is 3g / m 2 , thickness is 12μm, pore size is 0.6μm, air permeability is 80L / m 2 ·s; the hot pressing temperature is 250°C, the time is 9s, and the pressure is 2MPa to obtain a high temperature resistant filter material.

[0091] Example 4

[0092] Tetrabutyl titanate, acetic acid (concentration of 0.9 mol / L) and anhydrous ethanol in a volume ratio of 1:1.6:4.8 were mixed, and magnetic stirring (speed of 500 r / min) was performed for 20 min to obtain a mixed solution; the mixed solution was evenly mixed with activated carbon in a volume ratio of 1:0.8 to obtain a mud material, and the mud material was calcined at 950°C for 4 h under a nitrogen atmosphere. The calcined product was crushed and passed through a 60-mesh sieve to obtain TiO2 / activated carbon powder.

[0093] Ammonium metavanadate and cerium nitrate hexahydrate in a mass ratio of 1:0.7 are added to deionized water at 70°C, and stirred for 4 hours to obtain a mixed solution with a mass concentration of 8%; TiO2 / activated carbon powder is added to the mixed solution (the mass ratio of TiO2 / activated carbon powder and mixed solution is 0.6:1) and mixed evenly to obtain mud, which is calcined at 450°C for 2 hours under a nitrogen atmosphere, and the calcined product is crushed and passed through a 60-mesh sieve to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst.

[0094] The multi-component composite catalyst was soaked in 0.1 mol / L sulfuric acid for 4 hours for acidification treatment, and then the composite catalyst was washed with deionized water until the pH value no longer changed. Then, the composite catalyst was dried in an oven at 100° C. for 12 hours to obtain an acidified composite catalyst.

[0095] The polyetheretherketone and the acidified composite catalyst are mixed and spun, and the fiber filaments are mixed, opened, combed, laid, needled, trimmed and wound to obtain a needle-punched felt. After the fiber filaments are laid, they are pre-needled to form a preliminary embryo felt. The pre-needling depth is 10 mm and the pre-needling density is 80 needles / cm 2After the pre-needling, the upper and lower needle-punching machines are used for the main needling to reinforce the needle-punched felt. The main needling depth is 6mm and the main needling density is 1100 needles / cm 2 ; Needle felt is used as the base of composite catalytic filter bag, with a total weight of 350g / m 2 .

[0096] The prepared acidified composite catalyst was placed in deionized water and subjected to ultrasonic oscillation (frequency of 100 Hz) for 2 h to obtain a catalyst suspension with a mass concentration of 2%. The needle felt was immersed in the catalyst suspension for 6 h and then dried at 80 ° C to obtain a catalyst-loaded needle felt. The catalyst loading of the needle felt was 85 g / m 2 .

[0097] A PTFE concentrated dispersion (the solid content of the PTFE concentrated dispersion is 60%), a stabilizer, sodium dodecyl sulfate, a foaming agent, an alkyl polyglycoside (APG), and deionized water are mixed (the mass ratio of the PTFE concentrated dispersion, the stabilizer, the foaming agent, and the deionized water is 1.5:0.05:0.6:97), and the mixed solution is foamed in a stirrer, and the stirrer stirs at a high speed of 3500r / min for 10 minutes to obtain a stable foam coating with a foaming ratio of 4:1; the foam coating is scraped on the upper and lower surfaces of the catalyst-loaded needle felt by a scraper (the thickness of the upper and lower surfaces is 0.5cm), and then a layer of PTFE microporous membrane is hot-pressed on the upper surface, and the gram weight of the PTFE microporous membrane is 3g / m 2 , thickness is 12μm, pore size is 0.6μm, air permeability is 80L / m 2 ·s; the hot pressing temperature is 250°C, the time is 9s, and the pressure is 2MPa to obtain a high temperature resistant filter material.

[0098] Example 5

[0099] This embodiment is the same as embodiment 4, except that the composite catalyst is acidified by soaking in 0.1 mol / L sulfuric acid for 5 hours.

[0100] Example 6

[0101] This embodiment is the same as embodiment 4, except that the composite catalyst is acidified by soaking in 0.1 mol / L sulfuric acid for 6 hours.

[0102] Comparative Example 1

[0103] This comparative example is the same as Example 4, except that the mixed solution and activated carbon are evenly mixed in a volume ratio of 1:0.8 and then directly dried at 100°C. After drying, the mixture is crushed and passed through a 60-mesh sieve, thereby omitting the step of high-temperature calcination in a nitrogen atmosphere.

[0104] Comparative Example 2

[0105] This comparative example is the same as Example 4, with the only difference being that the mixed solution and activated carbon are evenly mixed in a volume ratio of 1:0.8 and then directly dried at 100°C. After drying, they are crushed and passed through a 60-mesh sieve, thereby omitting the step of high-temperature calcination under a nitrogen atmosphere; at the same time, the acidification treatment step of the V2O5-CeO2-TiO2 / activated carbon multi-composite catalyst is omitted.

[0106] The performance of the high temperature resistant filter materials of the embodiments and comparative examples was tested.

[0107] The catalytic degradation performance of the high temperature resistant filter materials prepared in Examples 1 to 6 and Comparative Examples 1 to 2 was tested. The test method was as follows: o-dichlorobenzene with a molecular structure similar to dioxin was selected as a substitute for dioxin, and a micro-injection pump and a constant temperature oil bath were connected to a catalytic evaluation device, and the simulated gas distribution composition (volume ratio) was 11% O2 + 89% N2. 20 mL of o-dichlorobenzene was taken with a disposable medical syringe and placed on the micro-injection pump, the needle was connected to the air inlet pipe, and a constant temperature oil bath was placed under the air inlet pipe. The temperature was set to 200 ° C to convert liquid o-dichlorobenzene into gaseous state, so that it could be tested by the catalyst. The test started from 200 ° C, the heating rate was 5 ° C / min, and after heating at 200 ° C, 240 ° C, and 280 ° C for 20 minutes, an aluminum foil gas collection bag was used to collect gas, and then a 50 μL micro-injector was used to extract the gas from the two needle tubes from the gas collection bag and injected into a gas chromatograph for analysis. At the same time, the base peak area of ​​o-dichlorobenzene without catalyst was tested at 200°C, 240°C and 280°C, and the dioxin removal rate was calculated according to formula (1).

[0108]

[0109] In formula (1), A 基 and A 催 They are the baseline peak area and the peak area detected after using the catalyst, respectively.

[0110] The dioxin removal rates of the filter materials of the embodiments and comparative examples at different temperatures are shown in Table 1.

[0111] Table 1 Dioxin removal rates of the filter materials of the embodiments and comparative examples at different temperatures

[0112] Group Removal rate (200℃) Removal rate (240℃) Removal rate (280℃) Example 1 83.5% 82.7% 81.8% Example 2 86.2% 88.5% 86.7% Example 3 87.1% 88.1% 87.1% Example 4 88.1% 89.6% 88.8% Example 5 90.3% 89.7% 90.5% Example 6 92.1% 91.6% 90.8% Comparative Example 1 78.8% 77.6% 77.9% Comparative Example 2 66.7% 67.8% 66.3%

[0113] According to the results of Examples 1 to 6 and Comparative Examples 1 to 2, it can be seen that the catalytic degradation performance of the high temperature resistant filter material of the present invention on dioxins is less affected by temperature. According to the results of Examples 4 to 6, it can be seen that the catalytic degradation performance of the high temperature resistant filter material on dioxins is affected by the acidification time, and increasing the acidification time can increase the removal rate of dioxins by the material. According to the results of Examples 4 to 6 and Comparative Examples 1 to 2, it can be seen that the time of heat treatment and acidification treatment during the preparation of the high temperature resistant filter material has a greater impact on the catalytic degradation effect of dioxins.

[0114] The filtration performance of the high temperature resistant filter materials of Examples 1 to 4 was tested. The test method was as follows: the filtration performance of the samples was tested using the LZC-K1 filter material comprehensive performance test system. The test conditions were based on the European standard EN1822-3. The test flow range was 10 to 100 L / min, the measurement resistance range was 0 to 1000 Pa, and the test area was 100 cm 2 The test dust source is NaCl aerosol. The test shows that the filtration efficiency of the high temperature resistant filter material of Example 1 can reach up to 99.88%, the filtration efficiency of the high temperature resistant filter material of Example 2 can reach up to 99.78%, the filtration efficiency of the high temperature resistant filter material of Example 3 can reach up to 99.86%, and the filtration efficiency of the high temperature resistant filter material of Example 4 can reach up to 99.92%.

[0115] The high-temperature mechanical properties of the high-temperature resistant filter materials of Examples 1 to 4 were tested. The tensile test at high temperature was carried out according to the standard of normal temperature stretching. The experimental samples were placed in a testing machine with a high-temperature oven. When the high-temperature oven reached 250°C, the tensile test was carried out after keeping warm for 10 minutes to obtain high-temperature tensile data.

[0116] It is found through testing that after continuous high temperature aging at 250° C., the strength retention rate of the high temperature resistant filter materials of Examples 1 to 4 is greater than 90%.

[0117] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a high temperature resistant filter material, characterized in that: The following steps are included: 1) mixing tetrabutyl titanate, acetic acid, anhydrous ethanol and activated carbon to obtain a slurry; calcining the slurry to obtain TiO2 / activated carbon powder; 2) mixing ammonium metavanadate, cerium nitrate hexahydrate and water to obtain a mixed solution; adding TiO2 / activated carbon powder to the mixed solution to obtain a mud material; calcining the mud material to obtain a V2O5-CeO2-TiO2 / activated carbon multi-component composite catalyst; 3) acidifying, washing and drying the multi-component composite catalyst in sequence to obtain an acidified composite catalyst; 4) spinning the organic matter and the acidified composite catalyst, and then performing pre-needling and main needling in sequence to obtain a needle-punched felt; 5) subjecting the acidified composite catalyst and water to ultrasonic vibration to obtain a catalyst suspension; immersing the needle-punched felt in the catalyst suspension and drying it to obtain a catalyst-loaded needle-punched felt; 6) mixing the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water and foaming them to obtain a foam coating; 7) The foam coating is scraped onto the upper and lower surfaces of the catalyst-loaded needle-punched felt, and then a polytetrafluoroethylene microporous membrane is hot-pressed onto the upper surface of the needle-punched felt to obtain a high temperature resistant filter material.

2. The preparation method according to claim 1, characterized in that: Step 1) The volume ratio of tetrabutyl titanate, acetic acid and anhydrous ethanol is 1:1.2-2:4.4-5.5, and the volume ratio of the total volume of tetrabutyl titanate, acetic acid and anhydrous ethanol to the volume ratio of activated carbon is 1:0.8-1.2; The calcination temperature is 900-950° C., the calcination time is 2-4 hours, and the calcination atmosphere is a nitrogen atmosphere.

3. The preparation method according to claim 1 or 2, characterized in that: Step 2) the mass ratio of the ammonium metavanadate to the cerium nitrate hexahydrate is 1:0.6-0.8, and the mass concentration of the mixed solution is 2-10%; The mixing temperature is 60-80° C., the mixing time is 3-4 hours, the calcining temperature is 400-500° C., the calcining time is 2-4 hours, and the calcining atmosphere is a nitrogen atmosphere.

4. The preparation method according to claim 3, characterized in that: Step 3) The acidification reagent is sulfuric acid, the concentration of sulfuric acid is 0.08-0.12 mol / L, the acidification time is 4-6 hours, the washing reagent is water, and the pH value of the multi-component composite catalyst no longer changes; the drying temperature is 90-105° C., and the drying time is 12-18 hours.

5. The preparation method according to claim 4, characterized in that: Step 4) the mass ratio of the organic matter to the acidified composite catalyst is 10-30:70-90, and the organic matter comprises one or more of polyetheretherketone, polytetrafluoroethylene and polyphenylene sulfide; The depth of the pre-needling is 10-14 mm, and the density is 70-140 needles / cm 2 The main acupuncture depth is 6-12 mm, and the density is 1000-1500 needles / cm 2 .

6. The preparation method according to claim 4 or 5, characterized in that: Step 5) The mass concentration of the catalyst suspension is 1-8%, the immersion time is 6-8 hours, and the drying temperature is 80-100°C; The catalyst loading of the needle felt is 80 to 120 g / m 2 ; The total weight of needle felt is 200~600g / m 2 .

7. The preparation method according to claim 6, characterized in that: Step 6) The solid content of the polytetrafluoroethylene dispersion is 57-63%; the mass ratio of the polytetrafluoroethylene dispersion, the stabilizer, the foaming agent and water is 1.5-2: 0.05-0.1: 0.6-1: 97-98; The foaming time is 10 to 15 minutes, and stirring is performed during the foaming process at a stirring rate of 3000 to 5000 r / min; the foaming ratio of the foam coating is 4 to 6:1; The foaming agent is sodium cocoylamphoacetate or alkyl glucoside, and the stabilizer is Tween 80 or sodium lauryl sulfate.

8. The preparation method according to claim 7, characterized in that: Step 7) the thickness of the scraping is 0.4-0.6 cm; the temperature of the hot pressing is 200-300° C., the time of the hot pressing is 8-10 s, and the pressure of the hot pressing is 1-3 MPa; The weight of the polytetrafluoroethylene microporous membrane is 3 to 4 g / m 2 , thickness is 10-15μm, pore size is 0.6-0.8μm, air permeability is 70-100L / m 2 ·s.

9. The high temperature resistant filter material prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the high temperature resistant filter material according to claim 9 in removing dioxins.

Citation Information

Patent Citations

  • Filtering material possessing mercury removing efficacy and preparation method thereof

    CN105013246A

  • Preparation method of catalyst for combined emission reduction of NOx and dioxin

    CN109317134A

  • Preparation method and application of denitration, dioxin removal and dust removal three-in-one filtering material

    CN114130118A

  • Preparation method of noble metal nano-catalyst for removing dioxin

    CN115845873A

  • Adsorbing material for dioxin in flue gas and preparation method

    CN118320794A