Dry desulfurizer based on carbide slag as well as preparation method and application of dry desulfurizer

Through the combined molding technology of modified calcium carbide slag, metal oxides and binders, a dry desulfurizer with high porosity and strength was prepared, which solved the problem of low removal efficiency and powderization of calcium carbide slag, and achieved efficient desulfurization and resources Use.

CN118987960APending Publication Date: 2024-11-22JIZHI WISDOM (SHANGHAI) NEW TECH CO LTD
View PDF 0 Cites 1 Cited by

Patent Information

Application Number
CN202411285664.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-13
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, the dry desulfurization agent for calcium carbide slag has low efficiency in removing, and the pore structure is underdeveloped, resulting in powderization problems and is not suitable for large-scale resource utilization.

Method used

By mixing calcium carbide slag with tempering agents such as graphene, calcium carbonate, potassium carbonate, etc. to form modified calcium carbide slag, mixing it with metal oxide and binder and then drying it, it is prepared with high porosity and strength Dry desulfurization agent.

Benefits of technology

It improves the desulfurization efficiency and strength of the desulfurization agent, extends the effective desulfurization time, realizes large-scale resource utilization of calcium carbide slag, and reduces energy consumption and costs, making it suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005043049550000071
    Figure BDA0005043049550000071
Patent Text Reader

Abstract

The invention discloses a dry desulfurizer based on carbide slag as well as a preparation method and application of the dry desulfurizer. The preparation method comprises the following steps: 1) mixing carbide slag and a conditioning agent, and carrying out ball milling to obtain modified carbide slag; wherein the conditioning agent is selected from one or more of graphene, calcium carbonate, potassium carbonate, potassium bicarbonate and potassium hydroxide, and must contain graphene; the mass ratio of the carbide slag to the conditioning agent is (80-90): (10-20); the graphene accounts for 3-10 wt% of the conditioning agent in percentage by mass; 2) mixing 75-95 parts by weight of modified carbide slag, 5-15 parts by weight of a metal oxide and 2-8 parts by weight of a binder to obtain an initial mixture; (3) mixing the initial mixture with water, and molding to obtain a molded substance; and drying the molded product to obtain the dry desulfurization agent based on the carbide slag. The dry desulfurizer disclosed by the invention is high in porosity, relatively high in strength and relatively high in desulfurization efficiency, and large-scale resource utilization of the carbide slag can be realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a dry desulfurizing agent based on carbide slag, and a preparation method and application thereof. Background Art

[0002] On the one hand, the emission requirements for sulfur dioxide are becoming more and more stringent. On the other hand, carbide slag is a by-product formed in the process of producing polyvinyl chloride by the carbide method. The production of 1 ton of polyvinyl chloride emits about 1.5 to 1.9 tons of slurry (wet basis, 90% water content) of carbide slag. The actual annual production of polyvinyl chloride is about 300 million tons, so a large amount of carbide slag will be produced. As an industrial waste, carbide slag is usually landfilled or stored, which will pollute the water resources near the storage site and cause serious damage to the ecological environment. The main component of carbide slag is calcium hydroxide. The use of carbide slag desulfurization not only provides a desulfurizer for flue gas desulfurization, but also finds a reliable way out for carbide slag management, achieving the purpose of treating waste with waste, and has good social and economic benefits.

[0003] CN103752147A discloses a dry desulfurizer and a preparation method thereof, wherein the preparation method comprises: mixing 130 to 200 parts by weight of quicklime, 5 to 10 parts by weight of a modifier, and 350 to 450 parts by weight of wet carbide slag, sequentially performing a first stage of stirring and a second stage of reprocessing stirring to obtain a modified product; and drying the modified product to obtain a dry desulfurizer. The removal efficiency of the dry desulfurizer still needs to be further improved.

[0004] CN107673725A discloses a method for desulfurization based on carbide slag, comprising: adding a desulfurizer consisting of carbide slag, magnesium oxide and red mud to alkaline industrial wastewater to prepare a desulfurizer slurry; contacting the desulfurizer slurry with a specific flue gas; and discharging the slurry when the pH value of the absorption slurry reaches the range of 5.3 to 6.8 to obtain a desulfurized slurry. This method is a wet method for removing sulfur dioxide and is not suitable for dry fixed bed removal of sulfur dioxide.

[0005] CN110721571A discloses a dry desulfurizer for cement production and a preparation method thereof, wherein the dry desulfurizer comprises the following raw materials: 55-75% calcium-based material, 10-25% reducing agent, 1-10% catalyst, 0-10% auxiliary agent, and the calcium-based material comprises carbide slag. The desulfurization efficiency of the dry desulfurizer still needs to be improved, and the amount of carbide slag in the dry desulfurizer is small, and the desulfurizer is powdery and cannot be used in industrial applications.

[0006] CN114377541A discloses a method for preparing a low-temperature desulfurizer, which comprises: mixing a basic desulfurization material, an absorption aid, a catalytic component, an oxidizing component, a dispersing and expanding pore component, a lubricating component, and a binder in proportion, adding water to extrude strips, drying, and roasting to obtain the desulfurizer; the basic desulfurization material comprises one or more of calcium oxide, calcium hydroxide, calcium carbonate, and carbide slag; the absorbent comprises one or more of sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, sodium bicarbonate, and potassium bicarbonate; the catalytic component comprises one or more of iron oxide, copper oxide, manganese oxide, cobalt oxide, titanium dioxide, and rare earth oxides; and the oxidizing component comprises one or more of sodium hypochlorite, calcium hypochlorite, and sodium chlorate. The patent document uses many components and requires a roasting step, which results in high energy consumption and high cost. Summary of the invention

[0007] In view of this, one object of the present invention is to provide a method for preparing a dry desulfurizer based on carbide slag, wherein the prepared dry desulfurizer has high porosity, high strength, and high desulfurization efficiency, and can realize large-scale resource utilization of carbide slag. The preparation method is relatively simple to operate and has low energy consumption. Another object of the present invention is to provide a dry desulfurizer based on carbide slag prepared according to the preparation method as described above. Another object of the present invention is to provide the application of the dry desulfurizer based on carbide slag as described above.

[0008] On the one hand, the present invention provides a method for preparing a dry desulfurization agent based on carbide slag, comprising the following steps:

[0009] 1) mixing carbide slag and a conditioning agent, and ball milling to obtain modified carbide slag; wherein,

[0010] The conditioning agent is selected from one or more of graphene, calcium carbonate, potassium carbonate, potassium bicarbonate and potassium hydroxide, and must contain graphene; the mass ratio of carbide slag to conditioning agent is 80-90:10-20; the mass percentage of graphene in the conditioning agent is 3-10wt%;

[0011] 2) mixing 75 to 95 parts by weight of modified carbide slag, 5 to 15 parts by weight of metal oxide and 2 to 8 parts by weight of a binder to obtain an initial mixture;

[0012] 3) mixing the initial mixture with water and forming a molded product; drying the molded product to obtain a dry desulfurization agent based on carbide slag.

[0013] According to the preparation method of the present invention, preferably, the conditioning agent is selected from a plurality of graphene, potassium carbonate and potassium bicarbonate, and must contain graphene.

[0014] According to the preparation method of the present invention, preferably, the mass percentage of graphene in the conditioning agent is 4-8wt%.

[0015] According to the preparation method of the present invention, preferably, the ball milling is mechanical ball milling, using a mixture of large balls and small balls, the diameter of the large balls is 5-10 mm, the diameter of the small balls is 1-3 mm, and both the large balls and the small balls are zirconia balls.

[0016] According to the preparation method of the present invention, preferably, the ball-to-material ratio is 3 to 5:1, the rotation speed of the ball mill is 400 to 800 rpm, and the ball milling time is 1 to 3 hours.

[0017] According to the preparation method of the present invention, preferably, in step 2), the metal oxide is selected from at least one of iron oxide, magnesium oxide and aluminum oxide; and the binder is selected from at least one of kaolin, hydroxypropyl methylcellulose and citric acid.

[0018] According to the preparation method of the present invention, preferably, in step 3), the amount of water used is 20-40 wt % of the mass of the initial mixture.

[0019] According to the preparation method of the present invention, preferably, the drying temperature is 110-200° C., and the drying time is 1-5 h.

[0020] On the other hand, the present invention also provides a dry desulfurization agent based on carbide slag, which is prepared according to the preparation method as described above.

[0021] In another aspect, the present invention also provides a use of the above-described dry desulfurization agent based on carbide slag in fixed-bed dry removal of sulfur dioxide.

[0022] The dry desulfurizing agent based on carbide slag prepared by the present invention has high porosity and strength, high desulfurization efficiency and long effective desulfurization time. The present invention can make good use of carbide slag. The preparation method of the present invention does not use roasting, is relatively simple to operate, and is conducive to industrial application. DETAILED DESCRIPTION

[0023] The present invention is further described below in conjunction with specific embodiments, but the protection scope of the present invention is not limited thereto.

[0024] After extensive research and experiments, the present invention found that the pore structure of carbide slag is underdeveloped, resulting in low desulfurization efficiency when it is directly used, and the strength of the formed carbide slag desulfurizer is low, which is easy to produce pulverization during the operation of the desulfurization tower, which is not conducive to the large-scale resource utilization of carbide slag.

[0025] The preparation method of the dry desulfurizer based on carbide slag of the present invention comprises the following steps: (1) a step of forming modified carbide slag; (2) a step of mixing; and (3) a step of molding and drying.

[0026] <Formation steps of modified carbide slag>

[0027] The carbide slag and the conditioning agent are mixed and ball-milled to obtain modified carbide slag. The present invention finds that this method is beneficial to improving the pore structure of the carbide slag and improving the desulfurization efficiency.

[0028] The present invention uses calcium hydroxide contained in carbide slag as an active component, which not only reduces the pollution of waste slag to the environment and achieves waste treatment, but also greatly reduces the mining of limestone and reduces the carbon emission in the process of preparing slaked lime. Using carbide slag as the main component of the desulfurizer greatly saves operating costs and is conducive to the long-term continuous operation of the desulfurization system.

[0029] The present invention adopts the method of adding a conditioning agent and ball milling to enhance the porosity of carbide slag, effectively overcomes the disadvantage of underdeveloped pore structure of carbide slag, enables flue gas to enter the interior of the flue gas desulfurizer for reaction, and increases the reaction active sites.

[0030] In the present invention, the conditioning agent is selected from one or more of graphene, calcium carbonate, potassium carbonate, potassium bicarbonate and potassium hydroxide, and must contain graphene. Preferably, the conditioning agent is selected from multiple of graphene, calcium carbonate, potassium carbonate, potassium bicarbonate and potassium hydroxide, and must contain graphene.

[0031] According to one embodiment of the present invention, the conditioning agent is a mixture of graphene and potassium carbonate. According to another embodiment of the present invention, the conditioning agent is a mixture of graphene and potassium bicarbonate. According to yet another embodiment of the present invention, the conditioning agent is a mixture of graphene and potassium hydroxide.

[0032] In the present invention, the mass percentage of graphene in the conditioning agent is 3-10wt%, preferably 4-8wt%, and more preferably 5-7wt%, which is beneficial to improving the pore structure of carbide slag and improving the desulfurization efficiency.

[0033] In the present invention, the mass ratio of carbide slag to conditioning agent is 80-90:10-20, preferably 82-90:10-18, more preferably 85-90:10-15. This is conducive to improving the pore structure of carbide slag and improving desulfurization efficiency.

[0034] In the present invention, carbide slag and a conditioning agent are mixed, and the step of ball milling can specifically be: adding carbide slag and a conditioning agent into a ball mill respectively, and then ball milling.

[0035] In the present invention, the ball milling is mechanical ball milling, using a mixture of large balls and small balls, the diameter of the large balls is 5 to 10 mm, the diameter of the small balls is 1 to 3 mm, and both the large balls and the small balls are zirconia balls. The diameter of the large balls is preferably 5 to 8 mm, more preferably 5 to 6 mm. The diameter of the small balls is preferably 1 to 2 mm. The ratio of the number of large balls to small balls is about 1:2 to 3. For example, it can be 1:2.

[0036] The ball-to-material ratio (the ratio of the total mass of large balls and small balls to the total mass of carbide slag and conditioning agent) is 3 to 5:1, preferably 4 to 5:1, and more preferably 4.5 to 5:1. The rotation speed of the ball mill is 400 to 800 rpm, preferably 450 to 750 rpm, and more preferably 500 to 700 rpm. The ball milling time is 1 to 3 hours, preferably 1 to 2.5 hours, and more preferably 1 to 2 hours.

[0037] During ball milling, no additional solvent is needed, and no sieving is required after ball milling.

[0038] <Mixing Step>

[0039] 75-95 parts by weight of modified carbide slag, 5-15 parts by weight of metal oxide and 2-8 parts by weight of binder are mixed to obtain an initial mixture. The invention adopts metal oxide and modified carbide slag to be used in coordination, which is conducive to further improving the desulfurization effect and utilization rate of the dry desulfurizer.

[0040] In the present invention, the modified carbide slag can be 75 to 95 parts by weight, preferably 80 to 90 parts by weight, and more preferably 80 to 85 parts by weight. The metal oxide is selected from at least one of iron oxide, magnesium oxide and aluminum oxide, and is preferably selected from one of iron oxide, magnesium oxide and aluminum oxide. Iron oxide refers to ferric oxide. The metal oxide can be 5 to 15 parts by weight, preferably 8 to 15 parts by weight, and more preferably 10 to 15 parts by weight. The binder can be 2 to 8 parts by weight, preferably 4 to 8 parts by weight, and more preferably 5 to 7 parts by weight. The binder is selected from at least one of kaolin, hydroxypropyl methylcellulose (HPMC) and citric acid, and is preferably citric acid.

[0041] You can stir while mixing.

[0042] <Molding and drying steps>

[0043] The initial mixture is mixed with water and molded to obtain a molded product; the molded product is dried to obtain a dry desulfurizer based on carbide slag. This is conducive to obtaining a stable non-powdery dry desulfurizer, which is conducive to application.

[0044] In the present invention, the amount of water is 20-40wt% of the mass of the initial mixture, preferably 25-35wt%, more preferably 30-35wt%. When the initial mixture is mixed with water, it is sealed and stirred for 10-30 minutes. This is conducive to extrusion molding and to obtaining a desulfurizer with higher desulfurization efficiency.

[0045] In the present invention, the steps of mixing the initial mixture with water and forming the formed product specifically include: feeding the initial mixture into a kneading and forming system, adding water and stirring, and forming columnar particles by extrusion. The columnar particles have a length of 1 to 3 cm and a diameter of 4 to 5 mm.

[0046] In the present invention, the drying temperature can be 110-200°C, preferably 110-180°C, more preferably 120-180°C. The drying time can be 1-5h, preferably 1.5-4h, more preferably 2-3h. After drying, the product can be used for removing sulfur dioxide in fixed bed dry desulfurization.

[0047] The present invention also provides a dry desulfurization agent based on carbide slag prepared according to the preparation method as described above, which has high porosity, high strength, high desulfurization efficiency and long effective desulfurization time. The dry desulfurization agent based on carbide slag of the present invention can be applied to the fixed bed dry removal of sulfur dioxide.

[0048] <Analysis and testing methods>

[0049] The test methods used in the following examples are described as follows:

[0050] Sulfur dioxide removal experiment: Testo 340 was used to detect sulfur dioxide concentration. A simulated fixed bed reaction device was used at a temperature of 140°C, an oxygen content of 10 vol%, a moisture content of 3%, and a SO2 concentration of 200 mg / m 3 , reaction space velocity 800h -1 After the reaction was stable for 10 hours, the final instantaneous removal efficiency of SO2 was calculated by detecting the concentration of SO2 at the outlet.

[0051] Among them, desulfurization efficiency = ((total SO2 content in raw gas - total SO2 content in tail gas) / total SO2 content in raw gas) × 100%.

[0052] Determination method of porosity of dry desulfurizer: The porosity is determined by the porosity determination method in JB / T 8133.15-2013 standard, and the porosity is calculated according to the following formula:

[0053]

[0054] Where V is the sample volume, in cm 3; m is the mass of the sample, in g; m1 is the mass of the weighing bottle, in g; m2 is the mass of the boiled sample and the weighing bottle, in g; m3 is the mass of the boiled sample in water, in g; d0 is the volume density of water, in g / cm 3 .

[0055] Method for determining the strength of dry desulfurizer: Use YHKC-2A particle strength tester to test the strength of desulfurizer.

[0056] In the following examples, unless otherwise specified, the "parts" are parts by weight.

[0057] Example 1

[0058] 90 parts of carbide slag, 5 parts of potassium carbonate and 5 parts of graphene were added to a ball mill for mechanical ball milling. The mechanical ball milling adopts a mixture of large balls and small balls, the diameter of the large balls is 5 mm, the diameter of the small balls is 1 mm, the material of the large balls and the small balls is zirconium oxide, the ball-to-material ratio is 5:1, the ball milling is carried out at room temperature, the speed of the ball mill is 500 rpm, the ball milling time is 1 hour, and the solid powder after ball milling is the modified carbide slag.

[0059] 85 parts of modified carbide slag, 10 parts of iron oxide and 5 parts of citric acid obtained as above were added into a mixer and mixed to obtain an initial mixture.

[0060] 30 wt% of water is added to the initial mixture, the mixture is sealed and stirred for 20 minutes, and then extruded to obtain a columnar shaped object. The shaped object is placed in an oven, dried at 120° C. for 2 hours, and cooled to obtain columnar particles of dry desulfurizer based on carbide slag.

[0061] Example 2

[0062] 85 parts of carbide slag, 10 parts of potassium bicarbonate and 5 parts of graphene were added to a ball mill for mechanical ball milling. The mechanical ball milling adopts a mixture of large balls and small balls, the diameter of the large balls is 5 mm, the diameter of the small balls is 1 mm, the material of the large balls and the small balls is zirconium oxide, the ball-to-material ratio is 5:1, the ball milling is carried out at room temperature, the speed of the ball mill is 700 rpm, the ball milling time is 2 hours, and the solid powder after ball milling is the modified carbide slag.

[0063] 80 parts of modified carbide slag, 15 parts of iron oxide and 5 parts of citric acid obtained as above were added into a mixer and mixed to obtain an initial mixture.

[0064] 35 wt% of water of the initial mixture mass is added to the initial mixture, the mixture is sealed and stirred for 20 minutes, and then extruded to obtain a columnar molding. The molding is placed in an oven, dried at 180° C. for 2 hours, and cooled to obtain columnar particles of dry desulfurizer based on carbide slag.

[0065] Comparative Example 1

[0066] The only difference from Example 1 is that the modified carbide slag is replaced by unmodified carbide slag.

[0067] Table 1

[0068] serial number Porosity of desulfurizer % Strength of desulfurizer N Desulfurization efficiency% Example 1 41 150 96 Example 2 40 172 99 Comparative Example 1 30 79 68

[0069] It can be seen from Table 1 that the dry desulfurizer prepared by the present invention has a high desulfurization efficiency, a high strength and a high porosity, and can realize the large-scale resource utilization of carbide slag.

[0070] The present invention is not limited to the above-mentioned embodiments. Without departing from the essential content of the present invention, any deformation, improvement and substitution that can be conceived by those skilled in the art shall fall within the scope of the present invention.

Claims

1. A method for preparing a dry desulfurizer based on carbide slag, It is characterized in that The steps include: 1) mixing carbide slag and a conditioning agent, and ball milling to obtain modified carbide slag; wherein, The conditioning agent is selected from one or more of graphene, calcium carbonate, potassium carbonate, potassium bicarbonate and potassium hydroxide, and must contain graphene; the mass ratio of carbide slag to conditioning agent is 80-90:10-20; the mass percentage of graphene in the conditioning agent is 3-10wt%; 2) mixing 75 to 95 parts by weight of modified carbide slag, 5 to 15 parts by weight of metal oxide and 2 to 8 parts by weight of a binder to obtain an initial mixture; 3) mixing the initial mixture with water and forming a molded product; drying the molded product to obtain a dry desulfurization agent based on carbide slag.

2. The preparation method according to claim 1, It is characterized in that The conditioning agent is selected from a plurality of graphene, potassium carbonate and potassium bicarbonate, and must contain graphene.

3. The preparation method according to claim 1, It is characterized in that The mass percentage of graphene in the conditioning agent is 4-8wt%.

4. The preparation method according to claim 1, It is characterized in that The ball mill is a mechanical ball mill, which adopts a mixing method of large balls and small balls, the diameter of the large balls is 5-10 mm, the diameter of the small balls is 1-3 mm, and the large balls and the small balls are both zirconia balls.

5. The preparation method according to claim 4, It is characterized in that The ball-to-material ratio is 3 to 5:1, the rotation speed of the ball mill is 400 to 800 rpm, and the ball milling time is 1 to 3 hours.

6. The preparation method according to claim 1, It is characterized in that In step 2), the metal oxide is selected from at least one of iron oxide, magnesium oxide and aluminum oxide; and the binder is selected from at least one of kaolin, hydroxypropyl methylcellulose and citric acid.

7. The preparation method according to claim 1, It is characterized in that In step 3), the amount of water used is 20-40 wt % of the mass of the initial mixture.

8. The preparation method according to claim 1, It is characterized in that The drying temperature is 110-200°C and the drying time is 1-5h.

9. A dry desulfurization agent based on carbide slag, It is characterized in that It is prepared according to the preparation method according to any one of claims 1 to 8.

10. Use of the carbide slag-based dry desulfurization agent according to claim 9 in fixed-bed dry removal of sulfur dioxide.

Citation Information

Cited By

  • Calcium-based solid waste slurry desulfurization agent, preparation method, desulfurization method, and soil remediation agent

    WO2026145753A1