Modified zeolite adsorbent for adsorbing cadmium as well as preparation method and application of modified zeolite adsorbent

By combining natural zeolite with disodium ethylenediaminetetraacetate and epoxy silane coupling agent, a modified zeolite adsorbent was formed, which solved the problem of poor cadmium removal effect of zeolite and achieved efficient cadmium ion adsorption and stability Improved performance, suitable for wastewater treatment and suitable for industrial applications.

CN118988252APending Publication Date: 2024-11-22HANGZHOU NORMAL UNIVERSITY

Patent Information

Application Number
CN202411247414.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-06
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing zeolites have poor effect on cadmium removal, which limits their application in water treatment projects.

Method used

By shaking and stirring the natural zeolite in an inorganic alkali solution and grafting reaction with disodium ethylenediaminetetraacetic acid and epoxy silane coupling agent, a modified zeolite adsorbent is formed, which enhances its adsorption ability to cadmium ions.

Benefits of technology

It significantly improves the adsorption efficiency and stability of divalent cadmium ions, is suitable for wastewater treatment, and is cheap and easy to obtain, and is suitable for industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988252A_ABST
    Figure CN118988252A_ABST
Patent Text Reader

Abstract

The invention discloses a modified zeolite adsorbent for adsorbing cadmium and a preparation method and application thereof.The preparation method comprises the steps that natural zeolite is oscillated and stirred in an inorganic alkali solution, then placed in a solution containing ethylenediamine tetraacetic acid disodium salt and an epoxy silane coupling agent, subjected to a grafting reaction, left to stand, filtered and subjected to heat treatment, and the modified zeolite adsorbent for adsorbing cadmium is obtained; and cleaning and drying to obtain the modified zeolite adsorbent. The epoxy silane coupling agent is prepared from one or more of gamma-glycidyl ether oxypropyl trimethoxy silane, gamma-glycidyl ether oxypropyl triethoxy silane and 2-(3, 4-cyclohexene oxide) ethyl trimethoxy silane, and the epoxy silane coupling agent is prepared from one or more of gamma-glycidyl ether oxypropyl trimethoxy silane, gamma-glycidyl ether oxypropyl triethoxy silane and 2-(3, 4-cyclohexene oxide) ethyl trimethoxy silane. Specific to the problem of poor cadmium adsorption effect, natural zeolite is taken as a raw material to load disodium ethylene diamine tetraacetate, an epoxy silane coupling agent is introduced to realize stable loading of chemical bonding, disodium ethylene diamine tetraacetate can generate coordination with cadmium ions, and high adsorption removal efficiency is realized.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, and in particular to a modified zeolite adsorbent for adsorbing cadmium, and a preparation method and application thereof. Background Art

[0002] Cadmium (Cd) is a non-essential trace element that exists naturally in the earth's crust and sedimentary rocks. It is often used in batteries, electroplating, pigments, coatings and plastic stabilizers. The widespread use of cadmium-based products in different fields, from sewage irrigation, fertilizer application, mining, smelting to fuel combustion emissions, has led to an increasing amount of cadmium in soil and water. Cadmium is a globally recognized Class I carcinogen and a common prominent toxin in pollution. Chronic cadmium exposure in any way will have adverse effects on the heart, lungs, bones, gonads, and especially the kidneys. Long-term low-level cadmium exposure can cause chronic obstructive pulmonary disease, emphysema and chronic renal tubular disease, as well as cardiovascular diseases such as atherosclerosis, and is also carcinogenic. According to the results of the first national soil pollution survey released in 2014, the national soil pollution point exceeded the standard rate of 16.1%, and inorganic pollutants accounted for 82.8% of the total pollutants. Among inorganic pollutants, cadmium ranked first with an exceeding rate of 7.0%, so solving the cadmium pollution problem is of great significance.

[0003] Zeolite, as an alkali metal aluminosilicate with a porous structure, is widely used in various fields as an important adsorbent. According to statistics from the International Zeolite Association (IZA), there are 46 natural zeolite minerals, and more than 250 synthetic zeolites, and this number is still increasing. The more common ones are clinoptilolite, mordenite, analcime, sodium zeolite, and heulandite. Compared with the layered structure of montmorillonite and bentonite, zeolite has a complete aluminosilicate skeleton, that is, a cage-like structure formed by interconnected tetrahedrons composed of three elements: silicon, aluminum, and oxygen. This framework structure and its rough and porous surface morphology determine that it has high adsorption and ion exchange properties. Zeolite can adsorb heavy metal ions in water. And because of its cheap and easy-to-obtain characteristics, it is widely used in the field of water treatment, but due to problems such as poor adsorption selectivity and low removal rate, its application scenarios in actual water treatment projects are limited. Therefore, it is considered to use modification and other methods to improve its original adsorption performance.

[0004] Disodium ethylenediaminetetraacetate (EDTA-2Na) is a good complexing agent with the chemical formula C 10 H 14N2Na2O8, due to its rich functional groups and unique structure, can form stable compounds with metal ions, calcium, magnesium, etc., so it is often used in the field of water treatment. However, due to the inconvenience of recycling and regeneration, it is subject to certain restrictions during use. Summary of the invention

[0005] The invention aims at the problem that zeolite has poor effect in removing cadmium element, and provides a modified zeolite adsorbent specially for cadmium-containing wastewater. Disodium ethylenediaminetetraacetic acid is used to modify natural zeolite, so that the adsorption effect on cadmium is greatly improved.

[0006] To achieve the above object, the technical solution adopted by the present invention is:

[0007] A method for preparing a modified zeolite adsorbent for adsorbing cadmium comprises the steps of:

[0008] Step 1, shaking and stirring the cleaned and ground natural zeolite in an inorganic alkaline solution, filtering and washing the zeolite to neutrality, and drying;

[0009] Step 2, placing the dried zeolite in a solution containing disodium ethylenediaminetetraacetate and an epoxy silane coupling agent, standing after grafting reaction, filtering, heat-treating, and then washing and drying to obtain the modified zeolite adsorbent;

[0010] The epoxy silane coupling agent includes one or more of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane.

[0011] The present invention specifically addresses the problem of poor cadmium adsorption effect. Natural zeolite is used as a raw material to load disodium ethylenediaminetetraacetate and an epoxy silane coupling agent. After the silane coupling agent functionalizes the surface of the zeolite, the epoxy group is combined with the carboxyl group of disodium ethylenediaminetetraacetate to achieve stable loading by chemical bonding. In the actual treatment of cadmium-containing wastewater, disodium ethylenediaminetetraacetate can produce a coordination effect with cadmium ions, thereby achieving efficient adsorption and removal efficiency. The modified zeolite and adsorption principle are as follows. Figure 1 shown.

[0012] The natural zeolite includes any one or more of natural clinoptilolite, mordenite, chabazite, erionite, phillipsite, heulandite, lanozelite, stilbite and analcime; the natural zeolite itself has good adsorbent conditions, a stable framework structure, and more pores, and can perform physical adsorption and ion exchange. At the same time, its easy availability and low cost also have great advantages for subsequent industrial applications, but its adsorption performance needs to be improved.

[0013] Preferably, the natural zeolite is natural clinoptilolite, the pore size of which is just suitable for the adsorption of divalent cadmium ions, and is suitable for adsorbing divalent cadmium ions in wastewater treatment.

[0014] The particle size of the natural zeolite is 80-100 meshes.

[0015] Preferably, the present invention selects epoxy silane coupling agent as a connector between zeolite and disodium ethylenediaminetetraacetate, which can make zeolite and disodium ethylenediaminetetraacetate produce stronger chemical bonding.

[0016] The inorganic base includes one or more of sodium hydroxide, potassium hydroxide and barium hydroxide.

[0017] In step 1, the mass concentration of the inorganic alkali solution is 10 to 200 g / L, and the oscillation stirring time is 1 to 6 hours; the inorganic alkali solution is used to remove the original impurities in the pores of the natural zeolite, dredge the pores to increase the specific surface area and improve the cation exchange capacity, thereby enhancing the original physical properties of the substrate and improving the adsorption capacity of the zeolite for divalent cadmium ions by changing the silicon-aluminum ratio ion exchange performance.

[0018] The volume ratio of the natural zeolite mass to the inorganic alkaline solution in step 1 is (10-20) g: (100-200) mL. This step is mainly to dredge the holes and channels in the zeolite. The treatment efficiency is good within this range and it is not easy to affect the zeolite framework.

[0019] In step 2, the mass volume ratio of zeolite to solution is 1g:5-20mL. Preferably, the mass volume ratio of zeolite to solution is 1g:10-20mL. Too little solution content leads to a decrease in the amount of disodium ethylenediaminetetraacetate combined with zeolite, and the adsorption effect is reduced.

[0020] In step 2, the mass concentration of disodium ethylenediaminetetraacetate in the solution is 1-5%, the mass concentration of the epoxy silane coupling agent is 1-5%, and the concentration ratio of disodium ethylenediaminetetraacetate to the epoxy silane coupling agent is 0.5-2:1.

[0021] In step 2, the epoxy silane coupling agent includes γ-glycidyloxypropyltrimethoxysilane (KH-560) and / or γ-glycidyloxypropyltriethoxysilane. Different types of epoxy silane coupling agents have different hydrolysis reaction rates.

[0022] The more disodium EDTA is, the better the adsorption effect of the prepared adsorbent is, but the actual production cost is higher; conversely, the adsorption effect of the prepared adsorbent is worse. The higher the concentration of disodium EDTA solution, the more complete its contact with zeolite, and the better the adsorption effect of the prepared adsorbent; but too high a concentration of disodium EDTA will also cause the surface of the zeolite to be covered with excessive disodium EDTA, thereby reducing the physical properties of the zeolite itself, such as specific surface area and pore volume, and reducing its adsorption effect. The higher the concentration of the silane coupling agent, the more sites for disodium EDTA to bind to the zeolite, but the fewer unbound carboxyl groups of disodium EDTA itself, and the worse the adsorption capacity. Conversely, the binding ability of disodium EDTA to the zeolite is worse.

[0023] Preferably, the mass concentration of disodium edetate in the solution is 1-3%, more preferably 1-2%, and even more preferably 1%.

[0024] Preferably, the mass concentration of the epoxy silane coupling agent in the solution is 0.5-3%, more preferably 0.5-2.5%, and even more preferably 1-2.5%.

[0025] In step 2, the grafting reaction is carried out at 90-120° C. with stirring for 4-12 hours, and the heat treatment is carried out at 100-200° C. for 2-12 hours. Such treatment conditions will not affect the crystal structure of the zeolite itself, and can also ensure the stable combination of the zeolite, disodium ethylenediaminetetraacetic acid and the silane coupling agent.

[0026] The invention also provides a modified zeolite adsorbent for adsorbing cadmium obtained by the preparation method, and the surface of the adsorbent is loaded with disodium ethylenediaminetetraacetate.

[0027] The invention also provides the use of the modified zeolite adsorbent in adsorbing cadmium-containing wastewater. The adsorbent has good adsorption efficiency for divalent cadmium ions and strong adsorption stability.

[0028] Preferably, the maximum adsorption capacity of the modified zeolite adsorbent for cadmium ions can reach 13.17 mg / g.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) The present invention provides a zeolite adsorbent modified with disodium ethylenediaminetetraacetate for cadmium-containing wastewater, wherein a silane coupling agent is introduced as a binder, and disodium ethylenediaminetetraacetate is combined with zeolite by chemical bonding, thereby greatly improving the adsorption efficiency of divalent cadmium ions. At the same time, the obtained adsorbent product has more stable performance than general modified materials and is convenient for use under various environmental conditions. At the same time, because the raw materials are cheap and easily available, it is very suitable for large-scale application in the field of wastewater treatment.

[0031] (2) The main raw materials used in the zeolite-based adsorbent of the present invention are zeolite and disodium ethylenediaminetetraacetate. Zeolite is a natural mineral material, which is green, environmentally friendly and easy to recycle. Using the adsorbent of the present invention for wastewater treatment will not cause secondary pollution.

[0032] (3) The preparation method of the adsorbent based on zeolite of the present invention has a simple process flow, is easy to operate, and is easy to promote in industry. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] Figure 1 It is a schematic diagram of the preparation of the adsorbent and the reaction formula of the adsorption process in the present invention.

[0034] Figure 2 This is the surface morphology of the natural zeolite raw material used in Example 1.

[0035] Figure 3 This is the surface morphology of the modified zeolite adsorbent prepared in Example 1. DETAILED DESCRIPTION

[0036] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with embodiment. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. Those skilled in the art can make modifications or equivalent substitutions based on the understanding of the technical scheme of the present invention without departing from the spirit and scope of the technical scheme of the present invention, and all should be included in the protection scope of the present invention.

[0037] The raw materials used in the following specific embodiments are all purchased from the market, and the natural zeolite used is clinoptilolite from Lingshou County, Shijiazhuang City, Hebei Province.

[0038] Example 1

[0039] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0040] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0041] (3) The dried zeolite particles in step (2) were added to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:10, and then γ-glycidyloxypropyltrimethoxysilane coupling agent was added dropwise to a concentration of 1%, and the reaction was stirred at 100°C for 8 hours. After standing, the zeolite particles were placed in an oven at 120°C for heat treatment for 2 hours, and then washed and dried to obtain the zeolite adsorbent. The preparation principle and structural schematic diagram of the three-dimensional structure are shown in FIG. Figure 1As shown, the natural zeolite is first oscillated with an inorganic base to load hydroxyl groups in the pores, and then combined with an epoxy silane coupling agent, and then connected to disodium ethylenediaminetetraacetate through the epoxy coupling agent.

[0042] The natural zeolite raw material and the final adsorbent were subjected to SEM scanning to observe the microscopic morphology. Figure 2 As shown, the modified zeolite adsorbent is Figure 3 As shown, it can be seen that there is obvious loading of disodium EDTA on the surface of zeolite.

[0043] The specific surface area and pore size data before and after modification are shown in Table 1. It can be seen that the specific surface area of ​​the zeolite modified with ethylenediaminetetraacetic acid and silane coupling agent is reduced, but it does not affect or reduce its adsorption effect on cadmium. On the contrary, it has an excellent adsorption effect on cadmium ions.

[0044] Table 1 Surface parameters of natural zeolite loaded with disodium EDTA

[0045]

[0046] Example 2

[0047] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0048] (2) Place 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shake and stir for 1 h. After standing, remove the supernatant, rinse the zeolite particles until the pH is neutral, and dry them;

[0049] (3) adding the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:20, then adding γ-glycidyloxypropyltrimethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 8 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0050] Example 3

[0051] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0052] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0053] (3) adding the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:5, then adding γ-glycidyloxypropyltrimethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 8 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0054] Example 4

[0055] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0056] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0057] (3) adding the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:10, then adding γ-glycidyloxypropyltrimethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 12 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0058] Example 5

[0059] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0060] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0061] (3) adding the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:10, then adding γ-glycidyloxypropyltrimethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 4 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0062] Example 6

[0063] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0064] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0065] (3) adding the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:10, then adding γ-glycidyloxypropyltriethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 4 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0066] Comparative Example 1 without EDTA-2Na

[0067] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0068] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0069] (3) adding the dried zeolite particles obtained in step (2) into deionized water, maintaining a zeolite mass to liquid volume ratio of 1:10, then adding γ-glycidyloxypropyltrimethoxysilane coupling agent dropwise to a concentration of 1%, maintaining the reaction at 100° C. with stirring for 4 h, filtering after standing, placing the zeolite particles in an oven at 120° C. for heat treatment for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0070] Embodiment 7-9

[0071] The preparation process is the same as that of Example 1, except that the concentration of the disodium ethylenediaminetetraacetic acid solution participating in the reaction is adjusted to 0.5%, 3%, and 5%.

[0072] Comparative Example 2: No silane coupling agent

[0073] (1) washing the natural zeolite, grinding and sieving to obtain 80-mesh zeolite particles, washing and drying for later use;

[0074] (2) placing 2 g of zeolite particles in a 200 g / L sodium hydroxide solution at room temperature and shaking and stirring for 1 h, removing the supernatant after standing, washing the zeolite particles until the pH is neutral, and drying;

[0075] (3) Add the dried zeolite particles obtained in step (2) to a 1% disodium ethylenediaminetetraacetic acid solution, maintaining a zeolite mass to solution volume ratio of 1:10, stirring and reacting at 100° C. for 8 h, leaving the mixture to stand and then filtering, heat treating the zeolite particles in an oven at 120° C. for 2 h, and then washing and drying to obtain the zeolite adsorbent.

[0076] Examples 10-12

[0077] The preparation process is the same as that of Example 1, except that the concentration of γ-glycidyloxypropyltrimethoxysilane participating in the reaction is adjusted to 0.5%, 2.5%, and 5%.

[0078] Comparative Example 3

[0079] The preparation process is the same as that of Example 1, except that the disodium ethylenediaminetetraacetic acid involved in the reaction is replaced with polyacrylic acid of equal mass.

[0080] Application Examples

[0081] The embodiment and the comparative example were tested for oscillating adsorption of divalent cadmium ions. The test steps were as follows: 0.5 g of zeolite adsorbent was placed in 100 mL, 10 mg / L divalent cadmium ion solution (cadmium chloride configuration), and the mixture was oscillated at a speed of 120 r / min and a constant temperature of 25 ° C for 8 h. The supernatant was taken for ICP detection to obtain the element concentration, and the divalent cadmium ion concentration C of the solution after adsorption was obtained by calculation. Fe (mg / L) and removal rate (%), the test results are shown in Table 1.

[0082] Table 1 Test results of oscillating adsorption of divalent cadmium ions in embodiments and comparative examples

[0083]

[0084] Example 1 has the best adsorption effect on divalent cadmium ions, with an adsorption rate of 99.32%. Examples 1 to 3 studied the effect of different zeolite mass and mass volume ratio of ethylenediaminetetraacetic acid disodium solution on the adsorbent's cadmium adsorption performance. From the results, it can be seen that the appropriate mass volume ratio in the preparation process is conducive to the improvement of the adsorption performance of the adsorbent, which can ensure the full contact between the zeolite particles and the ethylenediaminetetraacetic acid disodium, so that the reaction can be carried out more completely.

[0085] Examples 1, 4, and 5 show that appropriately extending the reaction time of zeolite particles and disodium ethylenediaminetetraacetic acid solution is beneficial to improving the adsorption performance of the adsorbent for divalent cadmium ions, but too long a reaction time will slightly reduce the treatment efficiency. Therefore, considering comprehensive economic factors, maintaining a reaction time of 8 hours is a better choice.

[0086] Observation of the adsorption results of Examples 1 and 6 shows that under the same raw material concentration and the same conditions, the adsorbents formed by the two when different epoxy-based silane coupling agents are used for reaction have similar adsorption effects. The reason is that the epoxy group in the silane coupling agent will undergo a ring-opening addition reaction with the carboxyl group on disodium ethylenediaminetetraacetate, thereby forming a chemical bond with the zeolite. The adsorbent formed when γ-glycidyloxypropyltrimethoxysilane is used has a better adsorption effect, and the reason may be that compared with the ethoxy group, the methoxy group in the silane coupling agent is more conducive to hydrolysis and condensation reactions, promoting the combination of disodium ethylenediaminetetraacetate and zeolite.

[0087] Observing the adsorption results of Example 1 and Comparative Example 1, when the substrate and other reaction conditions remain unchanged, the adsorption performance of the adsorbent prepared without disodium ethylenediaminetetraacetate participating in the reaction is greatly weakened. The reason is that the zeolite itself has a poor adsorption effect on divalent cadmium ions, and the excellent adsorption effect of the adsorbent on divalent cadmium ions mainly depends on the chelating ability of the functional groups contained in disodium ethylenediaminetetraacetate.

[0088] By observing Examples 7-9 again, it can be concluded that too high a concentration of disodium ethylenediaminetetraacetic acid solution participating in the reaction is not conducive to improving the adsorption performance of the adsorbent. The reason may be that when the concentration of disodium ethylenediaminetetraacetic acid in the solution is high, too much disodium ethylenediaminetetraacetic acid will cover the surface of the zeolite, which will weaken the physical properties of the zeolite itself, such as the specific surface area and pore volume, and weaken the contact area between the divalent cadmium ions and the adsorbent material, thereby resulting in a decrease in the adsorption effect.

[0089] By observing the adsorption results of Example 1 and Examples 10-12, it can be seen that when other reaction conditions remain unchanged, the presence of the silane coupling agent can effectively enhance the adsorption performance of the adsorbent, and at the same time, appropriately increasing the concentration of silane is helpful to improve the adsorption performance. The reason may be that the silane coupling agent can effectively combine the zeolite and disodium ethylenediaminetetraacetate through chemical bonds, and appropriately increasing the concentration of the silane coupling agent can also increase the amount of zeolite combined with disodium ethylenediaminetetraacetate, but too high a concentration of the silane coupling agent will combine and consume the carboxyl group of disodium ethylenediaminetetraacetate, reducing the number of functional groups that can participate in the chelation reaction, thereby reducing the adsorption performance of the adsorbent.

[0090] By observing the removal rates of Example 1 and Comparative Example 3, it can be concluded that when disodium ethylenediaminetetraacetate is replaced by polyacrylic acid of equal mass and having the same carboxyl functional group, the removal rate is significantly reduced to only 58.07%. This is because the unique structure of disodium ethylenediaminetetraacetate can chelate cadmium ions, thereby greatly improving its adsorption capacity for cadmium ions.

Claims

1. A method for preparing a modified zeolite adsorbent for cadmium adsorption, characterized in that: Includes steps: Step 1, shaking and stirring the cleaned and ground natural zeolite in an inorganic alkaline solution, filtering and washing the zeolite to neutrality, and drying; Step 2, placing the dried zeolite in a solution containing disodium ethylenediaminetetraacetate and an epoxy silane coupling agent, standing after grafting reaction, filtering, heat-treating, and then washing and drying to obtain the modified zeolite adsorbent; The epoxy silane coupling agent includes one or more of γ-glycidyloxypropyltrimethoxysilane, γ-glycidyloxypropyltriethoxysilane, and 2-(3,4-epoxycyclohexane)ethyltrimethoxysilane.

2. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: The natural zeolite includes any one or more of natural clinoptilolite, mordenite, chabazite, erionite, phillipsite, heulandite, lauzenite, stilbite and analcime; the particle size of the natural zeolite is 80-100 meshes.

3. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: The inorganic base includes one or more of sodium hydroxide, potassium hydroxide and barium hydroxide.

4. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: In step 1, the mass concentration of the inorganic alkali solution is 10 to 200 g / L, and the shaking stirring time is 1 to 6 hours; In step 1, the volume ratio of the mass of natural zeolite to the inorganic alkaline solution is (10-20) g: (100-200) mL.

5. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: In step 2, the mass volume ratio of zeolite to solution is 1 g:5-20 mL.

6. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: In step 2, the mass concentration of disodium ethylenediaminetetraacetate in the solution is 1-5%, the mass concentration of epoxy silane coupling agent in the solution is 1-5%, and the concentration ratio of disodium ethylenediaminetetraacetate to epoxy silane coupling agent is 0.5-2:

1.

7. The method for preparing a modified zeolite adsorbent for cadmium adsorption according to claim 1, characterized in that: In step 2, the grafting reaction is carried out at 90-120° C. with stirring for 4-12 hours; and the heat treatment is carried out at 100-200° C. for 2-12 hours.

8. A modified zeolite adsorbent for cadmium adsorption obtained according to the preparation method of claims 1-7.

9. Use of the modified zeolite adsorbent according to claim 8 in adsorbing cadmium-containing wastewater.

Citation Information

Patent Citations

  • Preparation method of nanomaterial-modified zeolite, and applications of zeolite in environment restoration

    CN106179197A

  • Lead-cadmium ion imprinted magnetic SBA-15 micro-particles and preparation method thereof

    CN110508262A

  • Zeolite adsorbent based on polyacrylic acid as well as preparation method and application of zeolite adsorbent

    CN117920157A

  • Modified Cyclodextrin / mesoporous Silica for Adsorbing Pb and Cd and Application Thereof

    US20210371302A1

Cited By

  • Seedling raising method of radix fici simplicissimae and application of seedling raising method

    CN119744666A

  • A method for raising seedlings of Prunus armeniaca and its application