Bismuth vanadate / bismuth tungstate composite acoustic catalyst as well as preparation method and application thereof

The heterostructure of bismuth vanadate/bismuth tungstate composite acoustic catalyst improves the separation efficiency of electron hole pairs, solves the problem of insufficient acoustic catalytic activity of BiVO4, and achieves efficient removal of tetracycline pollutants in wastewater, with low cost and environmental protection Friendly features.

CN118988290AInactive Publication Date: 2024-11-22LIAONING UNIVERSITY
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411082420.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-08
Publication Date
2024-11-22
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The prior art is inefficient in removing tetracycline pollutants in wastewater, has high cost and secondary pollution, and the acoustic catalytic activity of BiVO4 is limited by the degree of high light-induced recombination and insufficient surface adsorption characteristics.

Method used

BiVO4/Bi2WO6 composite material was prepared by hydrothermal synthesis using bismuth vanadate/bismuth tungstate composite acoustic catalyst to form a heterostructure to improve the separation efficiency of electron-hole pairs, thereby improving the efficiency of acoustic catalytic removal of tetracycline.

Benefits of technology

It significantly improves the efficiency of acoustic catalytic removal of tetracycline, achieves efficient pollutant removal, and has low cost and environmentally friendly characteristics.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118988290A_ABST
    Figure CN118988290A_ABST
Patent Text Reader

Abstract

The invention discloses a bismuth vanadate / bismuth tungstate composite acoustic catalyst as well as a preparation method and application thereof. The preparation method comprises the following steps: dissolving NH4VO3 and Na2WO4. 2H2O in a NaOH solution, uniformly mixing, slowly dropwise adding a Bi (NO3) 3.5 H2O solution, adjusting the pH value of the solution, uniformly stirring, transferring the mixed solution into a reaction kettle, carrying out a hydrothermal synthesis reaction, cooling to room temperature, carrying out suction filtration, washing, and drying to obtain the bismuth vanadate / bismuth tungstate composite acoustic catalyst BiVO4 / Bi2WO6. The composite material provided by the invention has a synergistic effect with potassium persulfate to remove tetracycline through ultrasonic catalysis, the removal efficiency is high, and the reaction time is short. By using the method, the removal rate of tetracycline can reach 94.59% under the ultrasonic condition for 120 minutes. The prepared composite material has larger surface area and smaller forbidden bandwidth, inhibits compounding of electron hole pairs, generates more active free radicals, and greatly improves the efficiency of removing tetracycline through sound catalysis.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of acoustic catalytic composite materials, and in particular relates to a bismuth vanadate / bismuth tungstate composite acoustic catalyst and a preparation method and application thereof. Background Art

[0002] In recent years, the pollution of environmental systems by antibiotic drug residues in wastewater has attracted worldwide attention due to the discharge of hospital / pharmaceutical factory wastewater, human and animal excrement into water. Among them, tetracycline is a typical antibiotic that has been widely used in human, veterinary and agricultural applications. However, residual tetracycline in wastewater poses environmental risks by inducing ecotoxicity and promoting antibiotic resistance. Therefore, it has become an urgent issue to decompose the antibiotic tetracycline in wastewater into non-toxic and harmless small molecules. There are processes such as adsorption, electrolysis, photocatalysis, and chemical oxidation for the removal of tetracycline from wastewater. However, these methods have disadvantages such as high cost, low efficiency, and secondary pollution.

[0003] Ultrasonic removal has attracted widespread attention due to its simple equipment requirements, high efficiency and convenient operation. During the ultrasonic process, cavitation forms bubbles and breaks, generating sonoluminescence (SL) and high temperature and high pressure, which in turn generate a large number of active free radicals to mineralize organic matter. Adding sonocatalysts can improve the sonocatalytic removal efficiency by generating more electron-hole pairs.

[0004] BiVO4 is a semiconductor material whose small band gap enables it to efficiently absorb visible light and generate the required electron-hole pairs for photocatalysis. Monoclinic scheelite BiVO4 has been shown to be an efficient photocatalyst with low manufacturing cost, low hazard, and good photostability, making it a promising material. However, the sonocatalytic activity of BiVO4 is limited by the high degree of photoinduced recombination and insufficient surface adsorption characteristics, resulting in low sonocatalytic efficiency. Summary of the invention

[0005] The present invention aims to provide a bismuth vanadate / bismuth tungstate composite sonocatalytic material, which utilizes bismuth vanadate and bismuth tungstate to form a heterojunction to improve the separation efficiency of electron-hole pairs, thereby improving the sonocatalytic removal of tetracycline pollutants.

[0006] The technical scheme adopted by the present invention is: a bismuth vanadate / bismuth tungstate composite acoustic catalyst, and the preparation method comprises the following steps: taking NH4VO3 and Na2WO4·2H2O, dissolving them in a NaOH solution, mixing them evenly, slowly dropping a Bi(NO3)3·5H2O solution, adjusting the pH value of the solution, stirring them evenly, transferring the mixed solution to a reactor for a hydrothermal synthesis reaction, cooling to room temperature, filtering, washing, and drying to obtain a bismuth vanadate / bismuth tungstate composite acoustic catalyst BiVO4 / Bi2WO6.

[0007] Furthermore, in the bismuth vanadate / bismuth tungstate composite acoustic catalyst BiVO4 / Bi2WO6, in terms of molar percentage, Bi2WO6 accounts for 10% to 60% of BiVO4 / Bi2WO6.

[0008] Furthermore, in molar ratio, NH4VO3:Na2WO4·2H2O:Bi(NO3)3·5H2O=1:(0.11~1.5):(1.22~4.0).

[0009] Furthermore, the pH of the solution is adjusted to 4.5-5.5.

[0010] Furthermore, the hydrothermal synthesis reaction is carried out at 175-185° C. for 22-26 hours.

[0011] The invention provides an application of a bismuth vanadate / bismuth tungstate composite sonic catalyst in catalytic removal of organic pollutants.

[0012] Furthermore, the organic pollutant is tetracycline.

[0013] Furthermore, the method is as follows: adding bismuth vanadate / bismuth tungstate composite acoustic catalyst into wastewater containing tetracycline and ultrasonicating.

[0014] Furthermore, the addition amount of the bismuth vanadate / bismuth tungstate composite sonic catalyst is 1.0-2.0 mg / mL, the initial concentration of tetracycline is 30-50 mg / L, the ultrasonic power is 500 W, and the ultrasonic time is 100-150 min.

[0015] Furthermore, potassium persulfate is added simultaneously.

[0016] Furthermore, the amount of potassium persulfate added is 0.5-2.0 mg / mL.

[0017] The beneficial effects of the present invention are:

[0018] In the present invention, Bi2WO6 has attracted much attention due to its excellent visible light photocatalytic activity, unique layered structure, high thermal stability and photochemical stability, and environmental friendliness. Bi2WO6 shows a visible light absorption edge at a wavelength of 470 nanometers, and its band gap is 2.8eV. Bi2WO6 is composed of a perovskite-like structure [WO4] 2- Layer sandwiched between two layers [Bi2O2] 2+ The structure between the layers is conducive to separating the photoexcited electron-hole pairs. The present invention significantly improves the sonocatalytic activity by forming a heterostructure of Bi2WO6 and BiVO4, thereby achieving a more efficient sonocatalytic process.

[0019] The bismuth vanadate / bismuth tungstate composite sonic catalytic material of the present invention utilizes the good catalytic performance of bismuth vanadate and bismuth tungstate, and their composite produces a synergistic effect, thereby improving the catalytic efficiency and reaction rate. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is the XPS spectrum of the prepared BiVO4 / Bi2WO6 composite material.

[0021] Figure 2 This is a diagram showing the effect of different molar percentages of BiVO4 / Bi2WO6 composite materials on the removal of tetracycline solution.

[0022] Figure 3 This is a diagram showing the effect of ultrasonic catalysis on the removal of tetracycline by BiVO4 / Bi2WO6 composite material (molar percentage 45%) and different amounts of potassium persulfate added. DETAILED DESCRIPTION

[0023] Example 1 Bismuth vanadate / bismuth tungstate composite acoustic catalyst (BiVO4 / Bi2WO6)

[0024] (I) BiVO4 / Bi2WO6 with a molar percentage of 10%

[0025] Bi(NO3)3·5H2O (592.40721 mg, 1.22 mmol) was weighed and dissolved in 2 mL of concentrated nitric acid, and then deionized water was added to dilute it to 20 mL. After magnetic stirring for a period of time, a clear solution A was obtained.

[0026] Weigh Na2WO4·2H2O (36.65076 mg, 0.11 mmol) and NH4VO3 (117.0 mg, 1.0 mmol), dissolve in 20 mL of 2 mol / L NaOH solution, stir evenly, and obtain a clear solution B.

[0027] Under continuous stirring, solution A was added dropwise to solution B to form a yellow solution, and then the pH value of the mixed solution was adjusted to 5 with 2 mol / L NaOH solution and stabilized, and magnetic stirring was continued for 30 min. The resulting mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven, dried at 60 ° C for 6 h, and then ground to obtain a molar ratio of n (Bi2WO6) :n (BiVO4 / Bi2WO6) =1:10, that is, a BiVO4 / Bi2WO6 composite material with a molar percentage of Bi2WO6 of 10%.

[0028] (ii) BiVO4 / Bi2WO6 with a molar percentage of 20%

[0029] Bi(NO3)3·5H2O (727.605 mg, 1.5 mmol) was weighed and dissolved in 2 mL of concentrated nitric acid, and then deionized water was added to dilute it to 20 mL. After magnetic stirring for a period of time, a clear solution A was obtained.

[0030] Weigh Na2WO4·2H2O (82.4675 mg, 0.25 mmol) and NH4VO3 (117.0 mg, 1.0 mmol), dissolve in 20 mL of 2 mol / L NaOH solution, stir evenly, and obtain a clear solution B.

[0031] Under continuous stirring, solution A was added dropwise to solution B to form a yellow solution, and then the pH value of the mixed solution was adjusted to 5 with 2 mol / L NaOH solution and stabilized, and magnetic stirring was continued for 30 min. The resulting mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven, dried at 60 ° C for 6 h, and then ground to obtain a molar ratio of n (Bi2WO6) :n (BiVO4 / Bi2WO6) =2:10, that is, a BiVO4 / Bi2WO6 composite material with a molar percentage of Bi2WO6 of 20%.

[0032] (III) BiVO4 / Bi2WO6 with a molar percentage of 30%

[0033] Bi(NO3)3·5H2O (900.28578 mg, 1.85714 mmol) was weighed and dissolved in 2 mL of concentrated nitric acid, then deionized water was added to dilute to 20 mL, and a clear solution A was obtained after magnetic stirring for a period of time.

[0034] Weigh Na2WO4·2H2O (141.42844 mg, 0.42857 mmol) and NH4VO3 (117.0 mg, 1.0 mmol), dissolve in 20 mL of 2 mol / L NaOH solution, stir evenly, and clarify to obtain solution B.

[0035] Under continuous stirring, solution A was added dropwise to solution B to form a yellow solution, and then the pH value of the mixed solution was adjusted to 5 with 2 mol / L NaOH solution and stabilized, and magnetic stirring was continued for 30 min. The resulting mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven, dried at 60 ° C for 6 h, and then ground to obtain a molar ratio of n (Bi2WO6) :n (BiVO4 / Bi2WO6) =3:10, that is, a BiVO4 / Bi2WO6 composite material with a molar percentage of Bi2WO6 of 30%.

[0036] (IV) BiVO4 / Bi2WO6 with a molar percentage of 45%

[0037] Bi(NO3)3·5H2O (1279.60705 mg, 2.63636 mmol) was weighed and dissolved in 2 mL of concentrated nitric acid, then deionized water was added to dilute to 20 mL, and after magnetic stirring for a period of time, a clear solution A was obtained.

[0038] Weigh Na2WO4·2H2O (270.00374 mg, 0.81818 mmol) and NH4VO3 (117.0 mg, 1.0 mmol), dissolve in 20 mL of 2 mol / L NaOH solution, stir evenly with a glass rod, and clarify to obtain solution B.

[0039] Under continuous stirring, solution A was added dropwise to solution B to form a yellow solution, and then the pH value of the mixed solution was adjusted to 5 with 2 mol / L NaOH solution and stabilized, and magnetic stirring was continued for 30 min. The resulting mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven, dried at 60 ° C for 6 h, and then ground to obtain a molar ratio of n (Bi2WO6) :n (BiVO4 / Bi2WO6) =4.5:10, that is, the BiVO4 / Bi2WO6 composite material with a molar percentage of Bi2WO6 of 45%.

[0040] (V) BiVO4 / Bi2WO6 with a molar percentage of 60%

[0041] Bi(NO3)3·5H2O (1940.28 mg, 4.0 mmol) was weighed and dissolved in 2 mL of concentrated nitric acid, then deionized water was added to dilute it to 20 mL, and a clear solution A was obtained after magnetic stirring for a period of time.

[0042] Weigh Na2WO4·2H2O (494.805 mg, 1.5 mmol) and NH4VO3 (117.0 mg, 1.0 mmol), dissolve in 20 mL of 2 mol / L NaOH solution, stir evenly, and clarify to obtain solution B.

[0043] Under continuous stirring, solution A was added dropwise to solution B to form a yellow solution, and then the pH value of the mixed solution was adjusted to 5 with 2 mol / L NaOH solution and stabilized, and magnetic stirring was continued for 30 min. The resulting mixture was transferred to a polytetrafluoroethylene reactor, placed in a forced air drying oven, and reacted at 180 ° C for 24 h; after cooling to room temperature, it was filtered, and the filter residue was rinsed three times with deionized water, and then washed three times with anhydrous ethanol. Finally, the product was placed in a vacuum drying oven, dried at 60 ° C for 6 h, and then ground to obtain a molar ratio of n (Bi2WO6) :n (BiVO4 / Bi2WO6) =6:10, that is, a BiVO4 / Bi2WO6 composite material with a molar percentage of Bi2WO6 of 60%.

[0044] (VI) Characterization

[0045] Figure 1 The XPS spectra of the synthesized samples BiVO4, Bi2WO6 and BiVO4 / Bi2WO6 (molar percentage of 45%) are shown in Figure 1. The XPS spectra show that BiVO4 / Bi2WO6 contains Bi, V, O, and W elements. The above XPS research results confirm that the composite material prepared by the present invention is composed of BiVO4 and Bi2WO6 nanoparticles.

[0046] Example 2 Effect of BiVO4 / Bi2WO6 Composite Materials on Catalytic Ultrasonic Removal of Tetracycline Solution (I) Effect of BiVO4 / FeVO4 Composite Materials with Different Molar Ratios on Ultrasonic Removal of Tetracycline

[0047] The method is as follows: 20 mg of BiVO4 / Bi2WO6 powder and 20 mL of 50 mg / L tetracycline (TET) solution are added to a conical flask to mix them, and then placed in an ultrasonic cleaner. The ultrasonic power is set to 500 W and ultrasonicated for 120 min under light-proof conditions. After the ultrasonication, the catalyst is filtered out with a filter head, and the absorbance is detected with an ultraviolet spectrophotometer. The data is recorded and saved. The removal rate of tetracycline can be calculated using formula (1).

[0048] Removal rate (%) = [(A0-A t ) / A0]×100%(1)

[0049] Where A0 is the initial absorbance of tetracycline, At is the absorbance after the tetracycline solution was removed after each experiment.

[0050] In addition, the removal rate of tetracycline solution is within its λ max = Calculated by absorbance at 350 nm.

[0051] The results are as follows Figure 2 As shown, when the molar ratio is 45%, the synthesized BiVO4 / Bi2WO6 catalyst has the best removal effect, and the removal rate can reach 71.44±1.60%. This is because the composite of bismuth vanadate and bismuth tungstate forms an S-type heterojunction, which can adjust its electronic structure and improve the disadvantage of high electron-hole recombination rate, thus improving the removal effect.

[0052] (II) Effect of BiVO4 / Bi2WO6 composite material and potassium persulfate on the removal of tetracycline solution by ultrasonic catalysis

[0053] The method is as follows: 30 mg of BiVO4 / Bi2WO6 powder (molar percentage of 45%) and 20 mL of 30 mg / L tetracycline solution are added to a conical flask to mix them, and then potassium persulfate is added to the conical flask, and the amount of potassium persulfate added is 10 mg, 20 mg, 25 mg, 30 mg, and 40 mg respectively; then it is placed in an ultrasonic cleaner, and the ultrasonic power is set to 500 W and ultrasonicated for 120 minutes under light-shielding conditions. After the ultrasonication ends, the catalyst is filtered out with a filter head, and the absorbance is detected with an ultraviolet spectrophotometer. The data are recorded and saved, and the removal rate of tetracycline can be calculated using formula (1).

[0054] The results are as follows Figure 3 As shown in the figure, with the increase of potassium persulfate concentration, the removal effect of tetracycline gradually increases. When the amount of potassium persulfate added is 60 mg, the removal rate of tetracycline can reach 94.59±0.72% in 120 minutes.

[0055] H + +S2O8 2- →HS2O8 - (2)

[0056] HS2O8 - →H + +SO4 2- +SO4 - (3)

[0057] H2O+SO4 - →H + + OH+SO4 2- (4)

[0058] As shown in the above formulas (2)-(4), the addition of K2S2O8 produces more active substances and significantly improves its removal rate. The experimental results show that the synergistic ultrasonic catalytic removal of tetracycline solution by bismuth vanadate / bismuth tungstate composite material and potassium persulfate has the characteristics of high removal efficiency, short reaction time and low cost.

Claims

1. A bismuth vanadate / bismuth tungstate composite acoustic catalyst, characterized in that: The preparation method of the bismuth vanadate / bismuth tungstate composite acoustic catalyst comprises the following steps: taking NH4VO3 and Na2WO4·2H2O, dissolving them in a NaOH solution, mixing them evenly, slowly dropping a Bi(NO3)3·5H2O solution, adjusting the pH value of the solution, stirring them evenly, transferring the mixed solution to a reactor for a hydrothermal synthesis reaction, cooling to room temperature, filtering, washing, and drying to obtain the bismuth vanadate / bismuth tungstate composite acoustic catalyst BiVO4 / Bi2WO6.

2. The bismuth vanadate / bismuth tungstate composite sonic catalyst according to claim 1, characterized in that: In the bismuth vanadate / bismuth tungstate composite acoustic catalyst BiVO4 / Bi2WO6, in molar percentage, Bi2WO6 accounts for 10% to 60% of BiVO4 / Bi2WO6.

3. The bismuth vanadate / bismuth tungstate composite sonic catalyst according to claim 1, characterized in that: More like Morby, NH4VO3:Na2WO4·2H2O:Bi(NO3)3·5H2O=1:(0.11~1.5):(1.22~4.0).

4. A bismuth vanadate / bismuth tungstate composite sonic catalyst according to claim 1, 2 or 3, characterized in that: The solution pH is adjusted to 4.5-5.5; the hydrothermal synthesis reaction is carried out at 175-185° C. for 22-26 hours.

5. Use of a bismuth vanadate / bismuth tungstate composite sonic catalyst as described in any one of claims 1 to 4 in catalytic removal of organic pollutants.

6. The use according to claim 5, characterized in that: The organic pollutant is tetracycline.

7. The use according to claim 6, characterized in that: The method is as follows: adding a bismuth vanadate / bismuth tungstate composite acoustic catalyst as described in any one of claims 1 to 4 into wastewater containing tetracycline, and ultrasonicating.

8. The use according to claim 7, characterized in that: The addition amount of the bismuth vanadate / bismuth tungstate composite sonic catalyst is 1.0-2.0 mg / mL, the initial concentration of tetracycline is 30-50 mg / L, the ultrasonic power is 500 W, and the ultrasonic time is 100-150 min.

9. The use according to claim 8, characterized in that: Potassium persulfate was added at the same time.

10. The use according to claim 9, characterized in that: The amount of potassium persulfate added is 0.5-2.0 mg / mL.

Citation Information

Patent Citations

  • BiVO4 / Bi2WO6 composite semiconductor material as well as hydrothermal preparation method and application thereof

    CN103191725A

  • Bi2WO6 / BiVO4 heterojunction composite photocatalyst, preparation method and application thereof

    CN105457625A

  • CuWO4 / Bi2WO6 compound as well as preparation method and application thereof

    CN113546639A

  • CoWO4 / Bi2WO6 composite acoustic catalyst as well as preparation method and application thereof

    CN113713802A

  • Preparation method and application of bismuth vanadate / copper tungstate composite acoustic catalyst

    CN117205938A