Egg yolk shell type composite molecular sieve and preparation method thereof, hydrofining catalyst and preparation method and application thereof
By using the egg yolk shell composite molecular sieve support and nano self-assembly method, the problems of high energy consumption and short catalyst life in the prior art are solved, and high efficiency is achieved The hydrodesulfurization of macromolecular sulfides can be removed and meet the low sulfur content requirements of the national VI standard.
Patent Information
- Application Number
- CN202411083943.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing hydrodesulfurization catalysts have problems such as increasing energy consumption and reducing catalyst life when increasing the reaction depth, and it is difficult to effectively remove macromolecular sulfides such as 4,6-DMDBT.
The SiO2/TiO2 composite material with a controllable shell and core structure was synthesized by nano-self-assembly method using egg yolk shell composite molecular sieve as a carrier, and Ni and Mo metals were uniformly loaded thereon to form NiMo/TS-1-Yolk- Shell SiO2 catalyst optimizes the pore structure and acidity and improves catalytic activity.
It has achieved efficient hydrodesulfurization reaction, with the maximum desulfurization rate reaching 98%, the sulfur content is less than 10ppm, which meets the requirements of the national VI standard, and the catalyst has excellent catalytic properties and long life.
Smart Images

Figure CN118988394A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of catalysts, and in particular to an egg yolk-shell type composite molecular sieve and a preparation method thereof, a hydrogenation refining catalyst and a preparation method and application thereof. Background Art
[0002] Hydrofining technology is an effective means to improve oil quality and mass produce clean oil in the petroleum refining industry. The depth of hydrodesulfurization can be improved to a certain extent by increasing the reaction temperature, reducing the reaction space velocity, and increasing the reactor volume, but it will increase energy consumption, reduce the life of the catalyst and the amount of crude oil processed. In contrast, the most economical and simple way is to develop a suitable high-activity hydrodesulfurization catalyst to achieve large-scale production of ultra-low sulfur and ultra-clean oil.
[0003] In recent years, mesoporous and microporous composite molecular sieves have gradually become a research hotspot in the field of catalytic hydrogenation. Mesoporous and microporous composite technology combines the pore advantages of mesoporous molecular sieves with the characteristics of microporous molecular sieves such as adjustable acidity and high hydrothermal stability, and has a dual-template pore distribution of micropores and mesopores. Commonly used synthesis methods include in-situ synthesis, pore wall crystallization, and nanoassembly. Mesoporous and microporous composite technology not only broadens the pore size of zeolite molecular sieves, but can also effectively reduce or avoid the diffusion resistance of large molecular sulfides in the pores, accelerate the mass transfer and reaction process of reactants and products, and its significantly enhanced acidity provides more options for the hydrodesulfurization reaction path and selectivity, showing a synergistic effect that single-component molecular sieves do not have.
[0004] CN113019440A discloses a method for preparing a hydrofining catalyst for ultra-deep desulfurization of diesel, wherein the catalyst uses Beta / Al-SBA-15 composite molecular sieve and alumina as carriers. The method first synthesizes the Beta / Al-SBA-15 composite molecular sieve, and then kneads, shapes, dries and roasts it with alumina dry rubber powder. The method mainly relies on mechanical mixing, which makes it difficult to give full play to the diffusion advantages of reactant molecules in the large pore structure of the mesoporous molecular sieve, and to achieve the adjustment of the acidity of the carrier material and the optimization of the pore structure. Summary of the invention
[0005] In order to solve the above problems in the prior art, the purpose of the present invention is to provide an egg yolk-shell composite molecular sieve and a preparation method thereof, a hydrorefining catalyst and a preparation method and application thereof. The egg yolk-shell composite molecular sieve has a controllable shell thickness and core size, and the hydrorefining catalyst has good catalytic hydrodesulfurization activity.
[0006] In order to achieve the above-mentioned object, according to the first aspect of the present invention, there is provided an egg yolk-shell type composite molecular sieve (Yolk-Shell SiO2), which has an inner core composed of TS-1 molecular sieve, a shell layer composed of silicon dioxide and a cavity between the inner core and the shell layer; the thickness of the shell layer is 3 to 26 nm, preferably 7 to 23 nm, the diameter of the inner core is ≤51 nm, preferably 3 to 41 nm; the size of the cavity is 24 to 75 nm, preferably 30 to 65 nm.
[0007] The size of the cavity refers to the distance between the inner core and the outer shell.
[0008] The egg yolk shell type composite molecular sieve of the invention has controllable shell size and core size, which is beneficial to uniform loading of active metals and free diffusion of macromolecular reactants.
[0009] In a preferred embodiment of the present invention, the specific surface area of the egg yolk shell composite molecular sieve is 500 to 700 m 2 ·g -1 , preferably 520-650nm; average pore diameter 4-9nm, preferably 5-8nm; pore volume 0.5-1.4cm 3 ·g -1 , preferably 0.6~1.2cm 3 ·g -1 According to this preferred excellent pore structure and larger specific surface area and pore volume, it is more conducive to the uniform loading of active metals on the egg yolk-shell type composite molecular sieve. In a preferred embodiment of the present invention, micropores exist in the egg yolk-shell type composite molecular sieve, and the pore size of the micropores is about 0.67nm.
[0010] In a preferred embodiment of the present invention, the total acid content of the egg yolk-shell composite molecular sieve is 35 to 96 μmol·g -1 , preferably 48 to 84 μmol·g -1 ; L acid content is 30~76μmol·g -1 , preferably 40 to 68 μmol·g -1 ; B acid content is 5~20μmol·g -1 , preferably 8 to 16 μmol·g -1 According to the preferred egg yolk-shell type composite molecular sieve with suitable acidity, it is more conducive to the uniform loading of active metal on the egg yolk-shell type composite molecular sieve, changes the interaction force between metal and carrier, improves the dispersion of active metal, and is conducive to improving the efficiency during catalysis.
[0011] In a preferred embodiment of the present invention, the SiO2 / TiO2 molar ratio in the egg yolk-shell composite molecular sieve is 30 to 400. According to such a preferred silicon-aluminum ratio, it is more conducive to improving the hydrodesulfurization reaction activity.
[0012] According to another aspect of the present invention, a hydrorefining catalyst is provided, which is denoted as NiMo / TS-1-Yolk-Shell SiO2. The carrier of the hydrorefining catalyst is the above-mentioned egg yolk-shell composite molecular sieve, and the oxide of Mo and the oxide of Ni are loaded on the carrier. The catalyst obtained by combining the egg yolk-shell composite molecular sieve with Mo and Ni of the present invention has excellent catalytic hydrogenation activity.
[0013] In a preferred embodiment of the present invention, the proportion of the Mo oxide in the hydrorefining catalyst is 10-20%, preferably 12-16%, by mass ratio. The proportion of the Ni oxide in the hydrorefining catalyst is 2-5%, preferably 3-4%. According to such a preferred loading amount, the catalytic performance is further improved.
[0014] According to another aspect of the present invention, there is also provided an application of the above-mentioned hydrotreating catalyst in diesel desulfurization and hydrogenation.
[0015] In particular, the application of hydrotreating using 4,6-DMDBT as a model compound.
[0016] The macromolecular sulfide 4,6-DMDBT has a large steric hindrance, and it is usually difficult to directly perform deep desulfurization on it in the prior art. The catalyst of the present invention has a suitable pore structure, so it can effectively eliminate the diffusion effect, and can further optimize the catalyst structure, adjust the acidity, and optimize the distribution of the active phase NiMoS-II by combining meso-micropores and introducing Ni and Mo metals to modify the pore structure.
[0017] In a preferred embodiment of the present invention, the conditions for applying the catalyst of the present invention to the hydrorefining of 4,6-DMDBT are as follows: temperature is 300-400°C, preferably 340-360°C; pressure is 4-10MPa, preferably 4-6MPa; hydrogen-oil ratio is 200-600:1, preferably 200-400:1; liquid hourly space velocity is 1-3h -1 , preferably 1.5 to 2.5 hours -1 .
[0018] In a preferred embodiment of the present invention, the amount of the hydrotreating catalyst of the present invention relative to the catalyzed substrate is 1:200-400, preferably 1:350-390, calculated by mass ratio.
[0019] According to another aspect of the present invention, there is also provided a method for preparing the above-mentioned egg yolk-shell type composite molecular sieve, comprising:
[0020] Step S1, preparing a first mixed solution with a first template, a silicon source, a titanium source, an alcohol, and water, and performing a crystallization treatment to obtain a TS-1 molecular sieve precursor emulsion;
[0021] Step S2, preparing a second mixed solution with an organosilane precursor, a second template, a pore-enlarging agent, ammonia water, and alcohol; the organosilane precursor comprises at least one hydrophilic silicon source and at least one hydrophobic silicon source; the mass ratio of the second template to the pore-enlarging agent is 1 to 0.25, preferably 0.8 to 0.3;
[0022] Step S3, mixing the TS-1 molecular sieve precursor emulsion and the second mixed solution, performing nano self-assembly, and then performing a first calcination to obtain the egg yolk-shell type composite molecular sieve.
[0023] In the preparation method of the present invention, suitable reagents are selected, especially silicon sources with different hydrophilicity / hydrophobicity, and suitable amounts of pore expanders and template agents are selected, so that the obtained egg yolk-shell composite molecular sieve has a suitable structure. When the amount of pore expander is too much, the shell thickness and core size of the composite molecular sieve will be greatly reduced, the mechanical strength will be weakened, resulting in the molecular sieve being broken and the morphology being changed; otherwise, a thicker core and shell will be formed, which is not conducive to the free diffusion of macromolecular reactants.
[0024] In a preferred embodiment of the present invention, in step S1, the first template comprises tetrapropylammonium hydroxide (TPAOH). In a preferred embodiment of the present invention, in step S1, the silicon source comprises ethyl silicate (TEOS) and / or tetramethyl silicate (TMOS). In a preferred embodiment of the present invention, in step S1, the titanium source comprises tetrabutyl titanate (TBOT) and / or titanium tetrachloride (TiCl4). In a preferred embodiment of the present invention, in step S1, the alcohol comprises isopropyl alcohol (IPA).
[0025] In a preferred embodiment of the present invention, in step S1, the mass ratio of the TPAOH to the TEOS is 1.1-1.5:1, preferably 1.2-1.4:1; the mass ratio of the IPA to the TEOS is 1.1-1.4:1, preferably 1.2-1.3:1. In a preferred embodiment of the present invention, in step S2, the mass ratio of the organosilane precursor to the TMB is 1:0.3-1.4, preferably 1:0.5-1.2; the mass ratio of the organosilane precursor to the ammonia water is 1:0.4-0.5, preferably 1:0.43-0.48; the mass ratio of the organosilane precursor to the alcohol is 1:12-13, preferably 1:12.5-12.8.
[0026] In a preferred embodiment of the present invention, the crystallization treatment is carried out at a temperature of 140 to 180° C., preferably 160 to 170° C., and the time is 3 to 4 days.
[0027] In a preferred embodiment of the present invention, in step S2, the alcohol includes ethanol and / or isopropanol.
[0028] In a preferred embodiment of the present invention, the hydrophilic silicon source includes TEOS and / or TMOS; the hydrophobic silicon source includes 1,2-bistriethoxysilylethane (BTSE) and / or 1,2-bistrimethoxysilylethane (BTME).
[0029] In a preferred embodiment of the present invention, the mass ratio of the hydrophilic silicon source to the hydrophobic silicon source is 0.9 to 1.2, preferably 0.94 to 1.0.
[0030] In a preferred embodiment of the present invention, in step S3, the temperature of the first calcination is 450-600°C, preferably 500-550°C, and the time is 4-6h. Preferably, before the first calcination, the material obtained by nano self-assembly is washed and dried. More preferably, the washing is performed by filtration using an alcohol solvent to wash the obtained material to neutrality. More preferably, after washing the material obtained after nano self-assembly, it is incubated in water. Preferably, the incubation temperature is 70°C, the time is 10-14h, and it is performed under stirring. After incubation, it is dried and then the first calcination is performed.
[0031] In the preparation method of the egg yolk-shell type composite molecular sieve of the present invention, the sol-gel method is adopted to synthesize the egg yolk-shell type structure through water culture, and etching and multiple deposition steps are not required, which saves the preparation process, and the obtained egg yolk-shell type composite molecular sieve has excellent catalytic performance after being prepared as a catalyst.
[0032] According to another aspect of the present invention, a method for preparing the above-mentioned hydrorefining catalyst is also provided, comprising: loading a Mo precursor solution and a Ni precursor solution on an egg yolk-shell type composite molecular sieve by an equal volume impregnation method, and then performing a second calcination treatment to obtain the hydrorefining catalyst. For the impregnation order of the Mo precursor solution and the Ni precursor solution, preferably, the Mo precursor solution is impregnated first, and then the Ni precursor solution is impregnated.
[0033] In a preferred embodiment of the present invention, the second calcination is carried out at a temperature of 400 to 600° C., preferably 500 to 550° C., and for a time of 4 to 6 hours.
[0034] In a preferred embodiment of the present invention, the Mo precursor solution includes ammonium heptamolybdate solution and sodium molybdate solution; and the Ni precursor solution includes nickel nitrate solution and nickel chloride solution. There is no special requirement for the concentration of the precursor solution.
[0035] The present invention adopts a nano self-assembly method to synthesize a mesoporous composite molecular sieve. The composite material has a controllable shell size and core size, an excellent pore structure, a large specific surface area and a pore volume, which is conducive to the uniform loading of active metals and the free diffusion of macromolecular reactants. The mesoporous composite molecular sieve has suitable acidity, changes the interaction force between the metal and the carrier, improves the dispersion of the active metal, and is conducive to the hydrofining reaction. The hydrofining catalyst prepared with the composite molecular sieve has excellent catalytic performance. The catalyst and the supporting process technology are used to carry out the hydrofining reaction of the macromolecular sulfide 4,6-DMDBT, and the maximum desulfurization rate can reach more than 98%, and the sulfur content is less than 10ppm, which meets the requirements of the National VI standard. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the wide-angle XRD spectrum of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1.
[0037] Figure 2 This is the N2- adsorption-desorption isotherm diagram of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1.
[0038] Figure 3 The pore size distribution diagram of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1 is shown.
[0039] Figure 4 This is the transmission electron microscope (TEM) spectrum of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1.
[0040] Figure 5 This is a high-magnification transmission electron microscope (HRTEM) spectrum of the NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst (sulfurized state) prepared in Example 1. DETAILED DESCRIPTION
[0041] In order to have a clearer understanding of the technical features, purposes and beneficial effects of the present invention, the technical solution of the present invention is now described in detail below, but it should not be construed as limiting the applicable scope of the present invention.
[0042] If the specific conditions are not specified in the examples, the conventional conditions or the conditions recommended by the manufacturer shall be followed. If the sources of the reagents, instruments or method instructions used in the examples of the present invention are not specified, they are all conventional products that can be purchased commercially or obtained from the applicant.
[0043] Example 1
[0044] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which includes the following steps:
[0045] 1. Preparation of yolk-shell composite molecular sieve
[0046] Step S1, in an ice water bath, TEOS, TPAOH, TBOT and H2O are mixed in a mass ratio of 17.7:15.2:1:4.4, and stirred continuously until the mixture is uniformly mixed; after being uniformly dissolved, the water bath temperature is adjusted to 70°C, stirring is continued for 3 hours, and 48g of isopropanol is added; the resulting solution is crystallized at 170°C for 4 days to obtain a TS-1 molecular sieve precursor emulsion for standby use;
[0047] Step S2, at room temperature, add the template agent CTAB and the pore-enlarging agent TMB to the ethanol aqueous solution in a mass ratio of 1:1, and stir until the mixture is uniform; drop 6.7 g of ammonia water into the above solution, and continue stirring for 0.5 to 1 h; slowly drop an organic silane precursor (a mixed solution of TEOS and BTSE, m TEOS / m BTSE =6.7:7.1) and stirred for 1-2h to obtain a second mixed solution;
[0048] Step S3, mixing the second mixed solution with the aforementioned TS-1 molecular sieve precursor emulsion, controlling the SiO2 / TiO2 molar ratio to be 50, and continuing to stir until the mixture is uniformly mixed; centrifuging the mixed solution and filtering and washing with ethanol, soaking the obtained solid in 1000-1200g of water for incubation, and slowly stirring for 10-12h; stopping stirring, waiting for the solution to separate into layers, taking out the lower layer of solid, drying at 80°C for 12h, calcining at 550°C for 6h, and cooling to room temperature to obtain a TS-1-Yolk-Shell SiO2 composite carrier;
[0049] 2. Preparation of Hydrotreating Catalyst
[0050] By using an equal volume impregnation method, 0.73 g of ammonium molybdate was dissolved in deionized water to prepare a solution, and the solution was used to impregnate a TS-1-Yolk-Shell SiO2 composite carrier (4 g), and ultrasonic dispersion was performed for 15 minutes, dried at 100°C for 12 hours, calcined at 550°C for 6 hours, and cooled to room temperature to obtain a catalyst loaded with Mo;
[0051] 0.54 g of nickel nitrate was prepared into an impregnation solution, and the solution was used to impregnate Mo / TYS. After the impregnation, the solution was dispersed ultrasonically for 15 minutes, dried at 100°C for 12 hours, and calcined at 550°C for 6 hours to obtain a NiMo supported hydrotreating catalyst, which was recorded as Cat-1.
[0052] Example 2
[0053] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 1, except that the ratio of CTAB to TMB is 0.5, and the catalyst is recorded as Cat-2.
[0054] Example 3
[0055] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 1, except that the ratio of CTAB to TMB is 0.4, and the catalyst is recorded as Cat-3.
[0056] Example 4
[0057] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 1, except that the ratio of CTAB to TMB is 0.3, and the catalyst is recorded as Cat-4.
[0058] Example 5
[0059] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 1, except that the ratio of CTAB to TMB is 0.2, and the catalyst is recorded as Cat-5.
[0060] Example 6
[0061] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 4, except that the SiO2 / TiO2 molar ratio is 30, and the catalyst is recorded as Cat-6.
[0062] Example 7
[0063] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 4, except that the SiO2 / TiO2 molar ratio is 40, and the catalyst is recorded as Cat-7.
[0064] Example 8
[0065] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 4, except that the SiO2 / TiO2 molar ratio is 100, and the catalyst is recorded as Cat-8.
[0066] Example 9
[0067] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 4, except that the SiO2 / TiO2 molar ratio is 200, and the catalyst is recorded as Cat-9.
[0068] Example 10
[0069] This embodiment provides a yolk-shell type NiMo / TS-1-Yolk-Shell SiO2 hydrorefining catalyst, the preparation process of which is the same as that of Example 4, except that the SiO2 / TiO2 molar ratio is 400, and the catalyst is recorded as Cat-10.
[0070] Comparative Example 1
[0071] A hydrotreating catalyst was prepared according to the method of Example 1, except that commercial alumina purchased was used as a carrier in the comparative example. The prepared NiMo / Al2O3 hydrotreating catalyst loaded with molybdenum and nickel was designated as Cat-11.
[0072] Comparative Example 2
[0073] A hydrotreating catalyst was prepared according to the method of Example 1, except that TEOS was used as the single silicon source in step S3 of the comparative example. The prepared hydrotreating catalyst loaded with molybdenum and nickel was recorded as Cat-12.
[0074] Comparative Example 3
[0075] A hydrotreating catalyst was prepared according to the method of Example 1, except that BTSE was used as the single silicon source in step S3 of the comparative example. The prepared hydrotreating catalyst loaded with molybdenum and nickel was recorded as Cat-13.
[0076] Comparative Example 4
[0077] A hydrotreating catalyst was prepared according to the method of Example 1, except that only metallic nickel was loaded in the comparative example. The prepared hydrotreating catalyst loaded with only nickel was designated as Cat-14.
[0078] Comparative Example 5
[0079] A hydrotreating catalyst was prepared according to the method of Example 1, except that only metallic molybdenum was loaded in the comparative example. The prepared hydrotreating catalyst loaded with only molybdenum was recorded as Cat-15.
[0080] The TS-1-Yolk-Shell SiO2 material prepared in Example 1 was tested and analyzed, and its wide-angle XRD results are as follows: Figure 1 As shown; its N2- adsorption-desorption isotherm is as follows Figure 2 Its pore size distribution is shown as Figure 3 As shown; the transmission electron microscope (TEM) spectrum of the TS-1-Yolk-Shell SiO2 composite molecular sieve prepared in Example 1 is as shown Figure 4 Its transmission electron microscopy spectrum is shown in Figure 5 shown.
[0081] From the pore size distribution diagram ( Figure 3 ) It can be seen that the composite molecular sieve synthesized by the present invention has three peaks at 2.2nm, 10nm and 20-40nm, respectively, of which the first peak is attributed to the self-assembly of CTAB; the second peak is attributed to the mesoporous channels assembled by CTAB micelles and further enlarged by the pore expander TMB; the third peak originates from the cavity formed by incubation with water, which indicates that the pores of the composite molecular sieve are radially ordered and three-dimensionally open.
[0082] The yolk-shell composite material synthesized by the present invention has radially oriented orderly pores, which are open and continuous, have openings on the shell surface, and are radially oriented on the sphere surface. Therefore, sulfur-containing compounds can effectively diffuse into or out of the multi-level porous composite material, thereby improving mass transfer capacity.
[0083] like Figure 5As shown, black filamentous stripes can be clearly observed, which are the active phase. The NiMoS-Ⅱ active phase has a high degree of sulfidation and exists in the form of a certain number of stacking layers, and has better catalytic activity. When the proportion of NiMoS-Ⅱ active phase is high, it is more conducive to the hydrodesulfurization reaction.
[0084] The specific surface area, pore diameter and pore volume of the hydrotreating catalysts prepared in the examples and comparative examples were measured. The results are shown in Table 1 below.
[0085] It can be seen from the data in Table 1 that in the technical solution of the present invention, the preferred SiO2 / TiO2 molar ratio is 100, and the preferred CTAB to TMB mass ratio is 0.3.
[0086] Table 1
[0087] Example <![CDATA[Specific surface area (m 2 ·g -1 )]]> <![CDATA[Pore volume (cm 3 ·g -1 )]]> Pore size (nm) Cat-1 517 0.67 5.6 Cat-2 542 0.79 6.3 Cat-3 560 0.84 6.8 Cat-4 598 1.01 7.3 Cat-5 527 0.85 7.5 Cat-6 514 0.60 6.5 Cat-7 552 0.63 7.1 Cat-8 642 1.21 7.6 Cat-9 537 0.95 8.0 Cat-10 466 0.93 8.3 Cat-11 266 0.74 8.6 Cat-12 357 0.48 4.0 Cat-13 189 0.33 3.2 Cat-14 530 0.73 6.6 Cat-15 527 0.70 6.1
[0088] The shell thickness and core size of the hydrotreating catalysts prepared in the examples and comparative examples were measured. The results are shown in Table 2 below.
[0089] Table 2
[0090]
[0091]
[0092] It can be seen from the data in Table 2 that in the technical solution of the present invention, as the CTAB / TMB mass ratio decreases, that is, the amount of TMB added increases, the shell thickness and the core size of the synthesized egg yolk shell type hydrorefining catalyst gradually decrease. When the CTAB / TMB mass ratio is too large, the shell thickness of the hydrorefining catalyst is thicker and the core size is larger; when the CTAB / TMB mass ratio is too small, the core of the hydrorefining catalyst tends to disappear.
[0093] When the SiO2 / TiO2 molar ratio of the composite molecular sieve is too low, that is, when the amount of TS-1 added is too much, the shell thickness increases significantly, while the core size remains almost unchanged. As the SiO2 / TiO2 molar ratio of the composite molecular sieve gradually increases, the shell size decreases, while the core size remains almost unchanged.
[0094] When only TEOS is used as the silicon source, the synthesized hydrotreating catalyst is a hollow structure without a core; when only BTSE is used as the silicon source, the synthesized hydrotreating catalyst is a solid sphere.
[0095] Using 4,6-DMDBT as a model compound, the hydrotreating reaction conditions were optimized and the raw material conversion rate, product distribution and yield were investigated. The results are shown in Table 3.
[0096] The reaction raw material is a 4,6-DMDBT-cyclohexane solution with a sulfur content of 500 ppm.
[0097] The specific test methods for the catalyst are as follows:
[0098] (1) Catalyst loading: quartz wool + quartz sand (20-40 mesh) 14 mL + quartz wool + refining agent 1 g + quartz wool + quartz sand 6 mL + quartz wool;
[0099] (2) Pre-sulfurization process conditions: temperature 340 °C, pressure 4 MPa, sulfide liquid flow rate 3 mL / h; stable for 4 hours;
[0100] (3) Evaluation process reaction conditions: reaction temperature 340°C, pressure 4 MPa, mass space velocity 1.5 h -1 , hydrogen-to-oil ratio 200:1.
[0101] Table 3
[0102]
[0103]
[0104] It can be seen from Table 3 that the hydrogenation effects of Cat-1 to Cat-10 on 4,6-DMDBT are higher than those of Comparative Examples 1-5 (Cat-11 to Cat-15), among which the desulfurization rate of Cat-8 on 4,6-DMDBT is higher than 98%, and the sulfur content of the product is lower than 10 ppm.
Claims
1. An egg yolk-shell composite molecular sieve, characterized in that: The egg yolk-shell composite molecular sieve comprises an inner core composed of TS-1 molecular sieve, a shell layer composed of silicon dioxide and a cavity between the inner core and the shell layer; the thickness of the shell layer is 3 to 26 nm; the diameter of the inner core is ≤51 nm; and the size of the cavity is 24 to 75 nm.
2. The egg yolk-shell type composite molecular sieve according to claim 1, characterized in that: The specific surface area of the egg yolk shell composite molecular sieve is 500 to 700 m 2 ·g -1 , preferably 520-650m 2 ·g -1 ; The average pore diameter is 4 to 9 nm, preferably 5 to 8 nm; Pore volume is 0.5~1.4cm 3 ·g -1 , preferably 0.6 to 1.2 cm 3 ·g -1 .
3. The egg yolk-shell type composite molecular sieve according to claim 1, characterized in that: The total acid content of the egg yolk-shell composite molecular sieve is 35 to 96 μmol·g -1 , preferably 48 to 84 μmol·g -1 ; L acid content: 30~76μmol·g -1 , preferably 40 to 68 μmol·g -1 ; B acid content: 5~20μmol·g -1 , preferably 8 to 16 μmol·g -1 .
4. The egg yolk-shell type composite molecular sieve according to claim 1, characterized in that: The molar ratio of SiO2 / TiO2 in the egg yolk-shell type composite molecular sieve is 30-400.
5. A hydrotreating catalyst, characterized in that: The carrier of the hydrotreating catalyst is the yolk-shell type composite molecular sieve according to any one of claims 1 to 4, and Mo oxide and Ni oxide are loaded on the carrier.
6. The hydrotreating catalyst according to claim 5, characterized in that In terms of mass percentage, the Mo oxide accounts for 10-20% in the hydrorefining catalyst, preferably 12-16%; the Ni oxide accounts for 2-5% in the hydrorefining catalyst, preferably 3-4%.
7. Use of the hydrotreating catalyst according to claim 5 or 6 in diesel desulfurization and hydrogenation.
8. The use according to claim 7, characterized in that: The invention comprises the application of the hydrofining catalyst to carry out hydrofining using 4,6-DMDBT as a model compound.
9. A method for preparing the egg yolk-shell type composite molecular sieve according to any one of claims 1 to 4, characterized in that: include: Step S1, preparing a first mixed solution with a first template, a silicon source, a titanium source, titanium tetrachloride, alcohol, and water, and performing a crystallization treatment to obtain a TS-1 molecular sieve precursor emulsion; Step S2, preparing a second mixed solution with an organosilane precursor, a second template, a pore-enlarging agent, ammonia water, and alcohol; the organosilane precursor comprises at least one hydrophilic silicon source and at least one hydrophobic silicon source; the mass ratio of the second template to the pore-enlarging agent is 1 to 0.25, preferably 0.8 to 0.3; Step S3, mixing the TS-1 molecular sieve precursor emulsion and the second mixed solution, performing nano self-assembly, and then performing a first calcination to obtain the egg yolk-shell type composite molecular sieve.
10. A method for preparing a hydrotreating catalyst according to claim 5 or 6, characterized in that: include: The precursor solution of Mo and the precursor solution of Ni are loaded on the yolk-shell type composite molecular sieve by using an equal volume impregnation method, and then a second calcination treatment is performed to obtain the hydrorefining catalyst.
Citation Information
Patent Citations
Method for preparing selective hydro-desulfurization catalyst
CN102091651A
Core / shell-type micropore / mesoporous composite titanium silicon molecular sieve and preparation method thereof
CN105712367A
Hierarchical pore monolithic molecular sieve catalyst and preparation method and application thereof
CN113813990A
Ordered mesoporous titanium-aluminum composite oxide coated TS-1 molecular sieve material and preparation method thereof
CN114669287A
Titanium silicate molecular sieve, and nano-gold-loaded titanium silicate molecular sieve catalyst and preparation method therefor and use thereof
WO2023116315A1