Cleaning method of boron diffusion quartz boat
Through the combined cleaning method of low-concentration acid solution, ammonia water and hydrogen peroxide, combined with ultrasonic and two-fluid spray technology, the problem of poor cleaning effect of boron diffusion quartz boat is solved, extending the life of the quartz boat and improving the cleaning efficiency, making it suitable for industrial applications.
Patent Information
- Application Number
- CN202411085055.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-08
- Publication Date
- 2024-11-22
AI Technical Summary
The existing boron diffusion quartz boat cleaning methods have problems such as poor cleaning effect, affecting the service life of the quartz boat, long cleaning time and high energy consumption.
The acid is used to pickle with a low-concentration mixed acid solution, and then ultrasonic soaked in a mixed solution of ammonia and hydrogen peroxide, combined with two-fluid spray cleaning and hot nitrogen drying, completely removing impurities and contamination on the quartz boat.
The complete removal of the quartz boat has been achieved, extending its service life, significantly improving the cleaning efficiency, and reducing cleaning time and energy consumption.
Smart Images

Figure BDA0004984942020000081 
Figure BDA0004984942020000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of solar cell manufacturing, and in particular to a method for cleaning a boron diffusion quartz boat. Background Art
[0002] The boron diffusion process is the process of preparing PN junctions in the manufacturing process of TOPCon solar cells. The quartz boat is used to repeatedly load silicon wafers and place them in the diffusion quartz furnace tube to complete the diffusion process. During the diffusion process, boron atoms are deposited on the surface of the silicon wafer mainly through the reaction of boron trichloride gas and oxygen at high temperature. In this process, intermediate products such as boron oxide and other by-products will be formed and attached to the quartz boat. In addition, since the silicon wafer needs to be repeatedly inserted and unloaded on the quartz boat, the frequent friction between the two will leave silicon powder on the boat teeth of the quartz boat. The long-term residue of boron oxide and silicon powder will pollute the quartz boat and eventually pollute the silicon wafer. In addition, during use, the quartz boat will also accumulate some organic impurities (mainly from the organic impurities such as lubricating oil accidentally contaminated by the silicon wafer during the transmission of the silicon wafer or the maintenance of the screw rod of the cleaning machine robot arm), resulting in cross-contamination of the silicon wafer.
[0003] In addition, the previous process of boron diffusion is a chemical cleaning process, and debris is prone to appear in the cleaning process. The debris is adsorbed on the normal wafer, resulting in the inability to effectively remove the surface liquid and various metal impurities, organic matter, and liquid on the surface of the silicon wafer. After entering the diffusion furnace, it will be burned. At the same time, the residue will contaminate the quartz boat. Subsequent production will cause continuous pollution to the silicon wafer, and ultimately lead to problems such as low battery efficiency and poor EL. Therefore, in order to ensure the stability of the efficiency and yield of TOPCon batteries, the quartz boat needs to be cleaned after long-term use or contamination.
[0004] At present, the boron diffusion quartz boat is mainly prepared by soaking the quartz boat in a 10%-30% HF solution for several hours (30-120 minutes), then putting the quartz boat into pure water and starting bubbling and overflow cleaning for 2 times, each time for 50-70 minutes, and finally using a nitrogen gun to blow dry the quartz boat before it is put into use. The disadvantages of this method mainly include the following aspects: (1) high concentration acid immersion will corrode the quartz boat, shorten the service life of the quartz boat, and it is not easy to rinse clean, which easily leads to acid residue, resulting in poor batch boat tooth marks. At the same time, the acid treatment cost is high; (2) the quartz boat cleaning quality is poor, and the quartz boat card slot or surface after cleaning still has dirt, liquid medicine, particles or heavy metal ions, which will eventually affect the electrical performance of the battery; (3) the long cleaning time limits the release of production capacity and increases the production and operation costs. Therefore, how to effectively clean the boron diffusion quartz boat without affecting the service life of the quartz boat and reducing the cleaning energy consumption is a bottleneck problem that needs to be solved urgently. Summary of the invention
[0005] In view of the problems of poor cleaning effect, affecting the service life of the quartz boat, long cleaning time and high energy consumption in the cleaning method of the boron diffusion quartz boat in the prior art, the present invention provides a cleaning method of the boron diffusion quartz boat. The present invention soaks the quartz boat in a low-concentration acid solution and then soaks it in a mixed solution of ammonia water and hydrogen peroxide. After washing, the card slot of the quartz boat is cleaned by two-fluid spray, and finally nitrogen drying is performed in a clean room, so that the impurities in the quartz boat are finally completely removed, and the whole cleaning process will not cause corrosion to the quartz boat, will not affect the service life of the quartz boat, and the cleaning efficiency is also significantly improved, which has a high value of promotion and application.
[0006] In order to solve the above technical problems, the technical solution provided by the present invention is:
[0007] A method for cleaning a boron diffusion quartz boat, the cleaning method comprising the following steps:
[0008] S1, placing the quartz boat to be cleaned into a low-concentration mixed acid solution for pickling, and after the pickling is completed, washing the quartz boat with bubbling overflow water to obtain a quartz boat I; the mixed acid solution is a mixed solution of HF and HCl;
[0009] S2, placing the quartz boat I in a mixed solution of ammonia water and hydrogen peroxide, heating, ultrasonically immersing, and then bubbling and overflowing water washing the quartz boat to obtain quartz boat II;
[0010] S3, using two-fluid spray to spray and clean the slot of the quartz boat II to obtain quartz boat III;
[0011] S4, placing the quartz boat III in a clean and closed drying device, introducing hot nitrogen gas to dry it, and obtaining a clean quartz boat.
[0012] Compared with the prior art, the cleaning method of the boron-diffused quartz boat provided by the present invention firstly uses a low-concentration mixed acid solution to pickle the quartz boat, wherein the quartz boat is slightly etched by a low-concentration HF solution to loosen and drop the silicon powder impurities on the surface of the quartz boat, and the metal ions adsorbed on the surface of the quartz boat for a long time are removed by low-concentration hydrochloric acid; then the quartz boat is cleaned by a mixed solution of ammonia water and hydrogen peroxide, wherein the heavy metal residues on the surface of the quartz boat are removed by the complexation of ammonia water, and the organic matter on the surface of the quartz boat is oxidized by hydrogen peroxide, and the metal ions adsorbed on the surface of the quartz boat are removed by the chelation of ammonia water. Ammonia water has a high affinity for organic matter, which promotes the rapid detachment of the oxidized oxide from the surface of the quartz boat, thereby effectively removing the residual organic matter. In addition, with the assistance of ultrasound, the large particle pollutants remaining on the surface of the quartz boat are removed more thoroughly. The dirt and liquid residues in the quartz boat slot that are difficult to remove are thoroughly removed by two-fluid spray. Finally, the quartz boat is dried in the cleaning chamber with hot nitrogen, which can effectively isolate the wet surface of the quartz boat from the outside world, avoid secondary contamination of the quartz boat surface during the drying process, and keep the quartz boat surface clean.
[0013] Furthermore, in step S1, the mass concentration of HF in the low-concentration mixed acid solution is 4% to 6%, and the mass concentration of HCl is 1% to 3%.
[0014] Furthermore, in step S1, the pickling time is 10 min to 30 min.
[0015] The process of the present invention adopts low-concentration mixed acid to pickle the quartz boat, and by limiting the ratio of HF to HCl and the pickling time, it can ensure that the residue on the surface of the quartz boat is cleaned and the quartz boat is not corroded. At the same time, the concentration of the mixed acid adopted by the present invention is low, and the residual acid on the surface of the quartz boat can be completely removed by subsequent bubbling overflow water washing after pickling, so that no acid residue is caused on the quartz boat, and secondary corrosion of the quartz boat by the residual acid after pickling is avoided.
[0016] Furthermore, in step S1, the time of the bubbling overflow water washing is 10 minutes to 30 minutes.
[0017] The fluidity of the cleaning liquid surface is increased by bubbling, and the detached pollutants are quickly removed from the cleaning tank by overflow, ensuring the cleanliness of the pure water tank and avoiding cross contamination.
[0018] It should be noted that in step S1, the temperature of the pickling and soaking is room temperature.
[0019] Furthermore, in S2, the mass concentration of the ammonia water in the mixed solution of the ammonia water and the hydrogen peroxide water is 4% to 6%, and the mass concentration of the hydrogen peroxide water is 4% to 6%.
[0020] Furthermore, in S2, the heating temperature is 50°C to 70°C.
[0021] Furthermore, in S2, the ultrasonic immersion time is 10 min to 20 min.
[0022] The quartz boat is cleaned with a mixed solution of ammonia and hydrogen peroxide in a specific ratio. By controlling the cleaning time and temperature, it can not only ensure the thorough removal of residual heavy metals and organic matter on the surface of the quartz boat, but also reduce the residual liquid on the surface of the quartz boat, avoiding the occurrence of problems such as unqualified cleaning of the quartz boat or excessive cleaning of the quartz boat that damages the quartz boat.
[0023] Furthermore, in S2, the time of the bubbling overflow water washing is 10 minutes to 30 minutes.
[0024] Bubble overflow cleaning can effectively remove residual liquid on the surface of the quartz boat, which is beneficial to reduce the quartz boat mark during normal production and improve the efficiency and yield of the battery cells.
[0025] Furthermore, in S3, the time of the spray cleaning is 1 min to 5 min.
[0026] It should be noted that when using two-fluid spray to clean the quartz boat slot, the two-fluid nozzle is placed above the quartz boat and aligned with the slot, and the two-fluid spray is repeatedly cleaned by reciprocating motion of the guide rail to completely remove dirt and particles in the slot.
[0027] Furthermore, in S4, the temperature of the hot nitrogen is 70° C. to 90° C., and the drying time is 10 min to 20 min.
[0028] As a specific embodiment of the present invention, a conventional quartz boat cleaning machine in the art can be used in S4 of the present invention. In order to achieve a clean environment, an air purifier is installed in the quartz boat cleaning machine. Specifically, the air purifier can be installed on the top cover of the drying tank, and the quartz boat to be cleaned can be placed in the drying tank.
[0029] The quartz boat is dried by hot nitrogen flow in the clean chamber to avoid secondary dust pollution after cleaning. Since the quartz boat is more likely to adsorb impurities after being wet, the present invention adopts hot nitrogen flow for drying. The hot nitrogen flow can effectively isolate the wet quartz boat from contact with the outside world, thereby ensuring the cleanliness of the surface of the quartz boat during the drying process.
[0030] The present invention adopts a low-concentration acid solution to soak the quartz boat, which will not corrode the quartz boat, thereby not affecting the service life of the quartz boat; and the low-concentration acid is easier to rinse, and will not cause acid residue on the surface of the quartz boat, thereby avoiding the occurrence of the problem of bad boat tooth marks in batches of quartz boats caused by residual acid; furthermore, the present invention adopts a mixed solution of ammonia water and hydrogen peroxide to effectively remove silicon powder residue and organic residue on the surface of the quartz boat, and cooperates with two-fluid spray to remove dirt and particles that are difficult to remove in the quartz boat slot, and finally achieves the purpose of removing residues from the quartz boat without dead angles, which is beneficial to improving the efficiency of boron diffusion battery cells and the product qualification rate, and the entire cleaning process is simple and the cleaning time is short. It is an efficient, green and environmentally friendly quartz boat cleaning method, suitable for industrial production applications, and has broad application prospects. DETAILED DESCRIPTION
[0031] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.
[0032] In order to better illustrate the present invention, further examples are given below.
[0033] In the following embodiments and comparative examples, the drying step after the quartz boat is cleaned adopts a quartz boat cleaning machine, and an air purifier is installed on the top of the drying tank of the quartz boat cleaning machine.
[0034] Example 1
[0035] This embodiment provides a method for cleaning a boron-diffused quartz boat, comprising the following steps:
[0036] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 20 minutes; wherein the mass concentration of HF in the mixed solution is 5%, and the mass concentration of HCl is 2%;
[0037] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0038] S3, placing the washed quartz boat in a mixed solution of NH4OH and H2O2, heating it to 60°C, turning on ultrasound, and soaking and cleaning it for 15 minutes; wherein the mass concentration of NH4OH in the mixed solution is 5%, and the mass concentration of H2O2 is 5%;
[0039] S4, place the quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0040] S5, placing the quartz boat on the workbench, placing the two-fluid spray on the guide rail above the quartz boat and aligning it with the quartz boat slot, and repeatedly cleaning the quartz boat slot for 2 minutes;
[0041] S6, putting the cleaned quartz boat into the drying tank of the quartz boat cleaning machine, passing 80° C. hot nitrogen gas for drying, the drying time is 15 minutes, taking it out, and obtaining a clean quartz boat.
[0042] Example 2
[0043] This embodiment provides a method for cleaning a boron-diffused quartz boat, comprising the following steps:
[0044] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 10 minutes; wherein the mass concentration of HF in the mixed solution is 6%, and the mass concentration of HCl is 3%;
[0045] S2, place the pickled quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 30 minutes;
[0046] S3, placing the washed quartz boat in a mixed solution of NH4OH and H2O2, heating it to 50°C, turning on ultrasound, and soaking and cleaning it for 20 minutes; wherein the mass concentration of NH4OH in the mixed solution is 4%, and the mass concentration of H2O2 is 4%;
[0047] S4, place the quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 10 minutes;
[0048] S5, placing the quartz boat on the workbench, placing the two-fluid spray on the guide rail above the quartz boat and aligning it with the quartz boat slot, and repeatedly cleaning the quartz boat slot for 1 minute;
[0049] S6, putting the cleaned quartz boat into the drying tank of the quartz boat cleaning machine, passing 90° C. hot nitrogen gas for drying, the drying time is 10 minutes, taking it out, and obtaining a clean quartz boat.
[0050] Example 3
[0051] This embodiment provides a method for cleaning a boron-diffused quartz boat, comprising the following steps:
[0052] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 30 minutes; wherein the mass concentration of HF in the mixed solution is 4%, and the mass concentration of HCl is 1%;
[0053] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 10 minutes;
[0054] S3, placing the washed quartz boat in a mixed solution of NH4OH and H2O2, heating it to 70°C, turning on ultrasound, and soaking and cleaning it for 10 minutes; wherein the mass concentration of NH4OH in the mixed solution is 6%, and the mass concentration of H2O2 is 6%;
[0055] S4, place the quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 30 minutes;
[0056] S5, placing the quartz boat on the workbench, placing the two-fluid spray on the guide rail above the quartz boat and aligning it with the quartz boat slot, and repeatedly cleaning the quartz boat slot for 5 minutes;
[0057] S6, putting the cleaned quartz boat into a drying tank of a quartz boat cleaning machine, introducing hot nitrogen at 70° C. for drying for 20 minutes, and taking it out to obtain a clean quartz boat.
[0058] Comparative Example 1
[0059] This comparative example provides a method for cleaning a boron-diffused quartz boat, comprising the following steps:
[0060] S1, place the quartz boat in a 15% HF solution and soak for 100 min;
[0061] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0062] S3, placing the quartz boat on a workbench, and using a compressed air gun to blow dry the water stains on the surface to obtain a cleaned quartz boat.
[0063] Comparative Example 2
[0064] This comparative example provides a method for cleaning a boron-diffused quartz boat, comprising the following steps:
[0065] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 120 minutes; wherein the mass concentration of HF in the mixed solution is 10%, and the mass concentration of HCl is 8%;
[0066] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0067] S3, putting the cleaned quartz boat into a drying tank of a quartz boat cleaning machine, passing hot air at a temperature of 80° C. for drying for 15 minutes, and taking it out to obtain the cleaned quartz boat.
[0068] Comparative Example 3
[0069] This comparative example provides a method for cleaning a boron-diffused quartz boat, which is different from Example 1 in that S3 and S4 are omitted, and specifically comprises the following steps:
[0070] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 20 minutes; wherein the mass concentration of HF in the mixed solution is 5%, and the mass concentration of HCl is 2%;
[0071] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0072] S3, placing the quartz boat on the workbench, placing the two-fluid spray on the guide rail above the quartz boat and aligning it with the quartz boat slot, and repeatedly cleaning the quartz boat slot for 2 minutes;
[0073] S4, putting the cleaned quartz boat into a drying tank of a quartz boat cleaning machine, introducing 80° C. hot nitrogen gas for drying for 15 minutes, and taking it out to obtain a clean quartz boat.
[0074] Comparative Example 4
[0075] This comparative example provides a method for cleaning a boron-diffused quartz boat, which is different from Example 1 in that the ammonia water is replaced with sodium hydroxide. The specific steps are as follows:
[0076] S1, placing the quartz boat in a mixed solution of HF and HCl and soaking for 20 minutes; wherein the mass concentration of HF in the mixed solution is 5%, and the mass concentration of HCl is 2%;
[0077] S2, place the acid-washed quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0078] S3, placing the washed quartz boat in a mixed solution of NaOH and H2O2, heating it to 60°C, turning on ultrasound, and soaking and cleaning it for 15 minutes; wherein the mass concentration of NaOH in the mixed solution is 2%, and the mass concentration of H2O2 is 5%;
[0079] S4, place the quartz boat in a pure water tank, open the overflow, and perform bubbling cleaning for 20 minutes;
[0080] S5, placing the quartz boat on the workbench, placing the two-fluid spray on the guide rail above the quartz boat and aligning it with the quartz boat slot, and repeatedly cleaning the quartz boat slot for 2 minutes;
[0081] S6, putting the cleaned quartz boat into a drying tank of a quartz boat cleaning machine, introducing 80° C. hot nitrogen gas for drying for 15 minutes, and taking it out to obtain the cleaned quartz boat.
[0082] The quartz boats cleaned in Examples 1 to 3 and Comparative Examples 1 to 4 were subjected to multiple boron diffusion tests. The silicon wafers after boron diffusion were put into the normal TOPCon battery production process, and battery efficiency and yield tracking experiments were carried out. The results are shown in Table 1.
[0083] Table 1
[0084]
[0085]
[0086] To sum up, the cleaning process of the boron-diffused quartz boat provided by the present invention can ensure that the residues on the surface of the quartz boat are cleaned, and will not cause corrosion to the quartz boat, will not affect the service life of the quartz boat, and will not form a slot mark after the boron diffusion of the silicon wafer, and will not have a poor appearance. At the same time, the quartz boat can be thoroughly cleaned, which is beneficial to improving the efficiency of the diffused battery cell and the product qualification rate. In addition, the cleaning time is greatly reduced, the efficiency is greatly improved, and then it is beneficial to increase production capacity. It is a new green and efficient quartz boat cleaning method with high practical value.
[0087] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modification, equivalent substitution or improvement made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A method for cleaning a boron-diffused quartz boat, characterized in that: The cleaning method comprises the following steps: S1, placing the quartz boat to be cleaned into a low-concentration mixed acid solution for pickling, and after the pickling is completed, washing the quartz boat with bubbling overflow water to obtain a quartz boat I; the mixed acid solution is a mixed solution of HF and HCl; S2, placing the quartz boat I in a mixed solution of ammonia water and hydrogen peroxide, heating, ultrasonically immersing, and then bubbling and overflowing water washing the quartz boat to obtain quartz boat II; S3, using two-fluid spray to spray and clean the slot of the quartz boat II to obtain quartz boat III; S4, placing the quartz boat III in a clean and closed drying device, introducing hot nitrogen gas to dry it, and obtaining a clean quartz boat.
2. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In step S1, the mass concentration of HF in the low-concentration mixed acid solution is 4% to 6%, and the mass concentration of HCl is 1% to 3%.
3. The method for cleaning a boron-diffused quartz boat according to claim 1 or 2, characterized in that: In step S1, the pickling time is 10 minutes to 30 minutes.
4. The method for cleaning a boron-diffused quartz boat according to claim 1 or 2, characterized in that: In step S1, the bubbling overflow water washing time is 10 minutes to 30 minutes.
5. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S2, the mass concentration of the ammonia water in the mixed solution of the ammonia water and the hydrogen peroxide water is 4% to 6%, and the mass concentration of the hydrogen peroxide water is 4% to 6%.
6. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S2, the temperature of the heating is 50°C to 70°C.
7. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S2, the ultrasonic immersion time is 10 min to 20 min.
8. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S2, the bubbling overflow water washing time is 10 minutes to 30 minutes.
9. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S3, the time of the spray cleaning is 1 min to 5 min.
10. The method for cleaning a boron-diffused quartz boat according to claim 1, wherein: In S4, the temperature of the hot nitrogen is 70° C. to 90° C., and the drying time is 10 min to 20 min.
Citation Information
Patent Citations
Method for cleaning quartz boat for diffusion
CN104741335A
Method for cleaning and saturating quartz boat for diffusion of crystalline silicon solar cell
CN113430652A
Method for cleaning and regenerating quartz part for semiconductor dry etching equipment
CN115591850A
Cited By
Method for cleaning quartz boat
CN121103795A