Medium-carbon free-cutting steel high-performance coiled cold-drawn material and preparation method thereof
Through hot-rolled disc round molding, slow cooling, light vibration treatment and cold drawing molding, the yield strength and surface quality of cold drawing materials of medium carbon easy-to-cut steel are improved, and the problem of insufficient yield strength in the existing technology is solved, satisfying the satisfaction of The performance requirements of high-end automotive parts.
Patent Information
- Application Number
- CN202410553224.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-07
- Publication Date
- 2024-11-22
AI Technical Summary
The yield strength of existing medium-carbon easy-to-cut steel cold-drawn materials is insufficient, which cannot meet the high-performance requirements of modern automobile manufacturing for high-end components.
The process of hot-rolled disc round molding, coil slow-cooling treatment, coil surface vibration treatment, coil cold-drawing molding treatment, cold-drawing straight strip aging and eddy current flaw detection treatment is adopted, and the heating temperature, cooling method, shot blasting current is controlled. and cold drawing speed to improve the yield strength and surface quality of steel.
The yield strength of cold-drawn medium-carbon easy-to-cut steel is significantly improved, reaching ≥695MPa, and ensuring that the surface is defect-free and meets the quality requirements of high-end automotive parts.
Smart Images

Figure CN118989030A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a cold-drawn material preparation technology for free-cutting steel, and more specifically to a medium-carbon free-cutting steel high-performance coil cold-drawn material and a preparation method thereof. Background Art
[0002] Free-cutting steel is widely used in the automotive industry, instrumentation, standard parts and other mechanical manufacturing industries due to its excellent cutting performance, high surface finish and high dimensional accuracy. Medium carbon free-cutting steel is a type of alloy steel.
[0003] Free-cutting steel coil cold-drawn material refers to free-cutting steel products produced by coil cold drawing technology.
[0004] The composition of medium carbon free-cutting steel is: C: 0.40-0.50wt%, Si: 0.20-0.40wt%, Mn: 1.30-1.70wt%, P: ≤0.030wt%, S: 0.20-0.40wt%, Cr≤0.15wt%, Ni: ≤0.10wt%, and the rest is Fe and unavoidable impurities and refined materials. It is made into free-cutting steel products through rolling and cold working.
[0005] At present, the production process of medium carbon free-cutting cold-drawn materials is: hot-rolled bars → annealing → cold-drawn finished products → straightening → packaging. The products produced by this process are rod-drawn products, which are suitable for low-end automobiles, mechanical equipment and other parts.
[0006] The cold-drawn products of medium carbon free-cutting steel produced by the above production process can meet the following product (ordinary grade) supply standards:
[0007] (1) Delivery status is in the form of cold drawn bars;
[0008] (2) Mechanical properties: Yield strength: 500-650MPa.
[0009] (3) Decarburization layer: The depth of decarburization layer of steel is ≤0.10mm.
[0010] The modern automobile manufacturing industry uses CNC machine tools as machining centers. The automation, precision and efficiency of machine tools place increasingly higher demands on the cutting performance of materials. At the same time, high-end automotive parts require very high mechanical properties, and the yield strength needs to be higher than 695MPa. However, the cold-drawn products of medium-carbon free-cutting steel produced by ordinary production processes can no longer meet the high performance requirements. Summary of the invention
[0011] The purpose of the present invention is to provide a medium carbon free-cutting steel high-performance coil cold-drawn material and a preparation method thereof. The high-performance coil cold-drawn material product of the medium carbon free-cutting steel prepared by the present invention has no surface cracking, effectively improves the mechanical performance index, and can meet the high-end demand of the market for automotive parts.
[0012] In order to achieve the above object, the present invention adopts the following technical solutions.
[0013] On the one hand, a medium carbon free-cutting steel high-performance coil cold-drawn material, comprising: C: 0.40-0.50wt%, Si: 0.20-0.40wt%, Mn: 1.30-1.70wt%, P: ≤0.030wt%, S: 0.20-0.40wt%, Cr≤0.15wt%, Ni: ≤0.10wt%, and the rest is Fe and inevitable impurities refined material, characterized in that:
[0014] The decarburized layer of the cold drawn material is ≤0.05 mm, and the yield strength of the mechanical property is ≥695 MPa.
[0015] On the other hand, the cold drawing method of the medium carbon free-cutting steel high-performance coil cold-drawn material comprises the following steps:
[0016] A. Hot rolled coil forming process: The billet is transformed into coil through heating, rolling, water tank cooling, and wire laying process, and a good hot rolled structure is obtained;
[0017] B. Slow cooling treatment of coils: The hot rolled coils are slowly cooled to reduce internal stress and restore plasticity;
[0018] C. Vibration treatment of coil surface: On the continuous cold drawing unit, a certain amount of deformation is taken to return to the roundness by shot blasting and vibration treatment;
[0019] D. Coil cold drawing process: On a continuous cold drawing machine, a single pass cold deformation of 20-35% is used to produce round coils into bars;
[0020] E. Aging and eddy current flaw detection of cold drawn straight bars: The cold drawn straight bars are placed at room temperature for a certain period of time to eliminate some internal stress. On the flaw detection equipment, the surface of the cold drawn finished straight bars is inspected one by one.
[0021] In step A, the heating furnace temperature of the hot rolled coil is controlled at 1160°C-1200°C, the billet rolling temperature is controlled at 1050°C-1100°C, a water tank is used for rapid cooling after rolling, the water tank flow rate is controlled at 20%-50%, and the spinning temperature is controlled at 800°C-850°C.
[0022] In step B, after spinning, the silk is slowly cooled through a heat preservation cover, and the temperature is controlled at 600-650° C. before entering the heat preservation cover to eliminate internal stress.
[0023] In step C, 1-3% deformation is adopted for shot blasting and vibration drawing to eliminate the blackened skin on the surface and return to roundness. 0.1mm cast steel shot is used for shot blasting, the shot blasting current is set to 6-10A, the shot blasting port is set to half-open state, and the cold drawing speed is 20-40m / min.
[0024] In step D, the parameters of the cold drawing die used to control the deformation amount include:
[0025] Inlet angle 60°, lubrication cone 16°, working cone 16°, sizing zone 0.2D-0.3D (D: nominal diameter) mm, outlet cone 60°; the material of the cold drawing die is YG8.
[0026] In step D, the following cold drawing speed parameters are used for control:
[0027] The cold drawing speed of free-cutting steel is controlled at 20-40m / min. At the same time, the angles of the horizontal and vertical axes of the mold are adjusted to maintain the straightness after cold drawing ≤2mm / m; the installation specification of the shearing die is the maximum size of the finished product + 0.5mm to ensure that the end is flat and there is no shearing indentation; the online pre-straightening of the finished product uses bidirectional straightening of the horizontal and vertical axes, and the straightness is ≤1mm / m; after polishing and two-roller fine straightening, the straightness is ≤0.5mm / m.
[0028] The medium carbon free-cutting steel high-performance coil cold-drawn material and its preparation method of the present invention, through the production mode of hot-rolled coil round forming treatment, coil slow cooling treatment, coil surface vibration light treatment, coil cold drawing forming treatment, cold drawn straight bar aging and eddy current flaw detection treatment, make the free-cutting steel meet the high-quality raw material requirements of surface quality without defects. Through the implementation of the cold processing technology, the comprehensive performance indicators of the product have been improved, especially the yield strength has been significantly improved, the surface quality has reached the defect-free level, and the raw material quality requirements of high-quality free-cutting steel of users have been met.
[0029] Invention drawings
[0030] Figure 1 It is a specific flow chart of the hot rolled coil forming process of the present invention;
[0031] Figure 2 It is a schematic diagram of the principle of coil cold drawing forming of the present invention. DETAILED DESCRIPTION
[0032] The composition of the medium carbon free-cutting steel high-performance coil cold-drawn material of the present invention includes: C: 0.40-0.50wt%, Si: 0.20-0.40wt%, Mn: 1.30-1.70wt%, P: ≤0.030wt%, S: 0.20-0.40wt%, Cr≤0.15wt%, Ni: ≤0.10wt%, and the rest is Fe and inevitable impurity refined material. The coil cold-drawn material also has the following characteristics:
[0033] (1) Delivery status is in the form of cold drawn bars;
[0034] (2) Its main performance requirements: decarburization layer ≤ 0.05 mm, mechanical properties yield strength: ≥ 695 MPa;
[0035] (3) Surface quality: There are no defects on the steel surface.
[0036] The preparation method of the medium carbon free-cutting steel high-performance coil cold-drawn material mainly comprises the following steps:
[0037] Hot rolled coil forming treatment, coil slow cooling treatment, coil surface vibration treatment, coil cold drawing forming treatment, cold drawn straight bar aging and surface flaw detection treatment, as follows:
[0038] 1. Hot rolled coil forming process: Figure 1 As shown, the billet is transformed into a coil through heating, rough rolling, water tank cooling, and wire laying processes in sequence, and a good hot rolling structure is obtained;
[0039] The blank is smoothly rolled into a round disc with a dense structure and no rolling defects on the surface. Due to the characteristics of the steel type, free-cutting steel is prone to cracking during rolling and requires a suitable rolling process. Therefore, the main process points of hot-rolled round disc forming are as follows:
[0040] The heating furnace temperature of the hot-rolled coil is controlled at 1160℃-1200℃, the billet rolling temperature is controlled at 1050℃-1100℃, and after rolling, a water tank is used for rapid cooling, the water tank controls the flow rate at 20%-50%, and the wire laying temperature is controlled at 800℃-850℃.
[0041] 2. Slow cooling treatment of coils: The hot-rolled coils are slowly cooled to reduce internal stress and restore plasticity. Specifically, after spinning, they can pass through several insulation covers in sequence. For example, a total of 26 insulation covers can be set. The first two insulation covers can be opened and controlled to 600-650℃ before entering the subsequent insulation covers to slowly cool and eliminate internal stress.
[0042] 3. Vibration treatment of coil surface: On the continuous cold drawing unit, a certain amount of deformation is adopted to return to roundness by shot blasting and vibration method. Specifically, on the continuous cold drawing unit with shot blasting machine, 1-3% deformation is adopted to carry out shot blasting and vibration cold drawing to eliminate the blackened skin on the surface and return to roundness.
[0043] Main process points: use 0.1mm cast steel shot, the shot blasting current is set to: 6-10A, the shot blasting mouth is set to: half-open state; cold drawing speed: 20-40m / min.
[0044] 4. Coil cold drawing: On a continuous cold drawing machine, a 20-35% deformation is used to produce round coils into bars. Figure 2 As shown, the process includes pre-straightening 1, cold drawing 2, cutting to length 3, finished product straightening 4, and bar collection 5. The cold drawing process specifically includes:
[0045] 1) Cold drawing production
[0046] Free-cutting steel is prone to cracking during cold working due to its high sulfur content, so the single-pass cold deformation is controlled in actual production. The single-pass cold deformation control range of this process is between 20-35%, ensuring smooth cold drawing and no cracking during the cold drawing process, thereby meeting high strength requirements.
[0047] 2) Mold requirements
[0048] Cold drawing is the key to ensure the dimensional accuracy and surface quality of the product. The important deformation tool used in cold drawing is the cold drawing die. Its quality requirements are: there are no defects such as sand holes, metal embedding, pits, annular grooves, etc. on the inner surface of the mold, and its surface finish reaches mirror finish.
[0049] The parameters used by the cold drawing die to control the deformation include:
[0050] Inlet angle 60°, lubrication cone 16°, working cone 16°, sizing zone 0.2D-0.3D (D: nominal diameter) mm, outlet cone 60°; the material of the cold drawing die is YG8.
[0051] 3) Cold drawing speed parameter control
[0052] The cold drawing speed of free-cutting steel is controlled at 20-40m / min. At the same time, by adjusting the angles of the horizontal axis (X axis) and the vertical axis (Y axis) of the die, the straightness after cold drawing is maintained at ≤2mm / m. The installation specification of the shear die is the maximum size of the finished product + 0.5mm to ensure that the end is flat and there is no shearing indentation; the finished product is pre-straightened online using the horizontal axis (X axis) and the vertical axis (Y axis) bidirectional straightening, and the straightness is ≤1mm / m; after polishing and two-roller fine straightening, the straightness is ≤0.5mm / m.
[0053] 5. Aging and eddy current flaw detection of cold-drawn bars: The cold-drawn bars are placed at room temperature for a certain period of time to eliminate some internal stress, which is conducive to subsequent user processing. On the flaw detection equipment, the surface of the cold-drawn finished bars is inspected one by one, and unqualified cold-drawn finished bars are automatically detected. The details are as follows:
[0054] The cold-drawn straight bars are placed at room temperature for more than two weeks, and the internal stress is released, which is convenient for later users to process and use. After the aging material, adjust the height of the eddy current flaw detection platform and replace the guide sleeve of the corresponding specification, adjust the distance between the probe and the test bar, adjust the front and rear drive wheels of the sensor system, keep the four wheels consistent in tightness, adjust the grating to ensure that the signal is correctly reflected when the bar passes through, and use the standard sample bar: the size of the artificial flaw on the flaw detection surface: 0.05×0.10×10mm (depth×width×length) for online flaw detection, and automatically detect defective products that do not meet the standard requirements.
[0055] By utilizing the work hardening of the material after cold drawing, the appropriate amount of deformation can achieve the required strength, which is beneficial to the high strength requirements of free-cutting steel, and the yield strength is ≥695MPa.
[0056] The following is a specific description through Examples 1-3. Table 1 shows the main chemical components of the medium carbon free-cutting steel produced in the three examples.
[0057] Table 1
[0058]
[0059] Among them, Example 1, specifically, hot rolling a 160 square billet into a Φ15 coil (heating temperature 1180°C, heating time 180 minutes, rolling temperature controlled at 1070°C, rapid cooling after rolling, water tank 30% flow, wire laying temperature 820°C) → slow cooling after rolling (open the first two insulation covers after wire laying, and all subsequent insulation covers are closed, and the temperature entering the insulation cover is controlled to be 620°C) → coil surface vibration light treatment (0.1 cast steel shot, shot blasting current setting: 8~10A, shot blasting port setting: half-open state, cold drawing speed: 25m / min) → coil cold drawing forming treatment into Φ13.2 rod (cold drawing speed 25m / min) → Φ13.2mm cold drawn straight bar is placed at room temperature for two weeks, and then eddy current flaw detection is performed online, and defective products with surface defects>0.05mm are automatically detected to produce qualified products.
[0060] Example 2, specifically, hot rolling a 160 square billet into a Φ15 coil (heating temperature 1170°C, heating time 170 minutes, rolling temperature controlled at 1075°C, rapid cooling after rolling, 30% flow in the water tank, and wire laying temperature 825°C) → slow cooling after rolling (open the first two insulation covers after wire laying, and all subsequent insulation covers are closed, and the temperature of the insulation cover is 625°C) → coil surface vibration light treatment (0.1 cast steel shot, shot blasting current setting: 8~10A, shot blasting port setting: half-open state, cold drawing speed: 25m / min) → coil cold drawing forming treatment Φ13 bar (cold drawing speed 25m / min) → Φ13mm cold drawn straight bars are placed at room temperature for two weeks, and then eddy current flaw detection is performed online, and defective products with surface defects>0.05mm are automatically detected to produce qualified products.
[0061] Embodiment 3: Specifically, 160 square billet is hot rolled into Φ14 coil (heating temperature 1190℃, heating time 180 minutes, rolling temperature is controlled at 1080℃, fast cooling after rolling, water tank 30% flow, wire laying temperature 830℃) → slow cooling after rolling (open two insulation covers after wire laying, and all insulation covers are closed subsequently, and the temperature of the insulation cover is 630℃) → coil surface vibration light treatment (0.1 cast steel shot, shot blasting current is set to: 8~10A, shot blasting port setting: half-open state, cold drawing speed: 30m / min) → coil cold drawing forming treatment Φ12.8 bar (cold drawing speed 30m / min) → Φ12.8mm cold drawn straight bar is placed at room temperature for two weeks, and then eddy current flaw detection is performed online, and defective products with surface defects>0.05mm are automatically detected to produce qualified products.
[0062] After testing, the properties of the rods produced in the above embodiments 1-3 are shown in Table 2:
[0063] Table 2
[0064]
[0065] In summary, the method for preparing high-performance coiled cold-drawn materials of medium-carbon free-cutting steel of the present invention has a smooth production process, can prepare high-performance coiled cold-drawn materials with no surface cracking, effectively improves the mechanical performance indicators, can meet the high-end demand of the market for automotive parts, and is suitable for mass production needs.
[0066] Those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention, and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.
Claims
1. A medium carbon free-cutting steel high-performance coil cold-drawn material, its composition include: C: 0.40~0.50wt%, Si: 0.20~0.40wt%, Mn: 1.30~1.70wt%, P: ≤0.030wt%, S: 0.20-0.40wt%, Cr≤0.15wt%, Ni: ≤0.10wt%, the rest is Fe and inevitable impurities refined material, characterized by: The decarburized layer of the cold drawn material is ≤0.05 mm, and the yield strength of the mechanical property is ≥695 MPa.
2. The method for preparing the medium carbon free-cutting steel high-performance coiled cold-drawn material according to claim 1, Features: The following steps are involved: A. Hot rolled coil forming process: The billet is transformed into coil through heating, rolling, water tank cooling, and wire laying process, and a good hot rolled structure is obtained; B. Slow cooling treatment of coils: The hot rolled coils are slowly cooled to reduce internal stress and restore plasticity; C. Vibration treatment of coil surface: On the continuous cold drawing unit, a certain amount of deformation is taken to return to the roundness by shot blasting and vibration treatment; D. Coil cold drawing process: On a continuous cold drawing machine, a single pass cold deformation of 20-35% is used to produce round coils into bars; E. Aging and eddy current flaw detection of cold drawn straight bars: The cold drawn straight bars are placed at room temperature for a certain period of time to eliminate some internal stress. On the flaw detection equipment, the surface of the cold drawn finished straight bars is inspected one by one.
3. The preparation method according to claim 2, Features: In step A, the heating furnace temperature of the hot rolled coil is controlled at 1160°C-1200°C, the billet rolling temperature is controlled at 1050°C-1100°C, a water tank is used for rapid cooling after rolling, the water tank flow rate is controlled at 20%-50%, and the spinning temperature is controlled at 800°C-850°C.
4. The preparation method according to claim 2, Features: In step B, after spinning, the silk is slowly cooled through a heat preservation cover, and the temperature is controlled at 600-650° C. before entering the heat preservation cover to eliminate internal stress.
5. The preparation method according to claim 2, Features: In step C, 1-3% deformation is adopted for shot blasting and vibration drawing to eliminate the blackened skin on the surface and return to roundness. 0.1mm cast steel shot is used for shot blasting, the shot blasting current is set to 6-10A, the shot blasting port is set to half-open state, and the cold drawing speed is 20-40m / min.
6. The preparation method according to claim 2, Features: In step D, the parameters of the cold drawing die used to control the deformation amount include: Inlet angle 60°, lubrication cone 16°, working cone 16°, sizing zone 0.2D-0.3D (D: nominal diameter) mm, outlet cone 60°; the material of the cold drawing die is YG8.
7. The preparation method according to claim 2, Features: In step D, the following cold drawing speed parameters are used for control: The cold drawing speed of free-cutting steel is controlled at 20-40m / min. At the same time, the angles of the horizontal and vertical axes of the die are adjusted to keep the straightness after cold drawing ≤2mm / m; The installation specification of the shearing die is the maximum size of the finished product + 0.5mm to ensure that the end is flat and there is no shearing indentation; the finished product is pre-straightened online using horizontal and vertical axis bidirectional straightening, with a straightness of ≤1mm / m; after polishing and two-roller fine straightening, the straightness is ≤0.5mm / m.
Citation Information
Patent Citations
High-performance hexagonal cold-drawn steel of S2 tool steel and production method thereof
CN102950445A
High strength level non-quenched-tempered steel bar for manufacturing of engine rocker and manufacture method thereof
CN110184527A
Rolling process for medium-carbon and high-sulfur alloy steel wire rod
CN111687209A
Production method of surface-defect-free type automobile suspension spring
CN115055531A
High-toughness free-cutting medium-carbon microalloyed steel and manufacturing method thereof
CN117144266A