Processing method for local conduction position of oxidized part
By machining reserved surfaces on mechanical parts and providing masking protection, the problem of masking misalignment during the oxidation process of the parts is solved, realizing an efficient machining method and reducing rework and costs.
Patent Information
- Application Number
- CN202411339067.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
During selective hard anodizing of mechanical parts, it is difficult to shield deep holes or small conductive surfaces, resulting in missing plating layers or misalignment of the shielding film, which increases rework and costs.
By machining a pre-reserved surface on the part, leaving a margin of 0.05mm, the oxide layer is removed after oxidation. Industrial tape is used for masking and protection, and residual adhesive is ground and the surface is cleaned to avoid masking misalignment.
Reduce worker workload, avoid missed plating or masking misalignment on conductive surfaces, improve surface quality, and ensure processing accuracy and efficiency.
Smart Images

Figure CN118989381A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of mechanical parts processing, and in particular to a method for processing a local conductive position of an oxidized part. Background Art
[0002] Some mechanical parts need to be selectively hard anodized to retain a portion of the conductive surface. In most cases, PE film is used to shield and protect the positions that do not need oxidation to prevent the surface from being oxidized. In the actual production process, parts have deep holes or small conductive surfaces that are difficult to shield. After oxidation, plating leakage or the movement of the masking film causes changes in the masking position, which leads to rework or multiple reworks that cause the parts to be scrapped, increasing costs. Therefore, a new technical solution is urgently needed to solve at least one of the above technical problems. Summary of the invention
[0003] The purpose of the present invention is to provide a processing method for the local conductive position of an oxidized part. By processing the reserved surface to leave a margin, even if there is an error in the thickness of the oxide layer, it can be removed in the secondary processing without any residue. There is no need to mask the conductive surface, which reduces the workload of workers and solves the problem of plating leakage or shielding offset on the conductive surface.
[0004] In order to achieve the above technical objectives and meet the above technical requirements, the technical solution adopted by the present invention is: a method for processing the local conductive position of an oxidized part, characterized in that it includes the following steps: Step 1: Drill the parts to obtain a reserved surface; Step 2, oxidizing the parts obtained in step 1; Step 3, shielding and protecting the bottom surface of the component obtained in step 2, removing the reserved surface obtained in step 2 and the oxide layer on the reserved surface, and obtaining a conductive surface; Step 4: clean the surface of the parts obtained in step 3.
[0005] As a preferred technical solution, the distance between the reserved surface and the conducting surface is 0.05 mm.
[0006] As a preferred technical solution, the specific steps of step 4 are: grinding to remove the masking residual glue remaining on the surface of the part, and degreasing and cleaning to remove the oily cutting fluid remaining on the surface of the part.
[0007] As a preferred technical solution, the oxidation in step 2 is specifically hard anodizing, and the bath liquid of the oxidation tank is a sulfuric acid solution or sulfuric acid with an organic acid added thereto.
[0008] As a preferred technical solution, the organic acid is oxalic acid or aminosulfonic acid.
[0009] As a preferred technical solution, the current density during oxidation in step 2 is 2-5A / dm².
[0010] As a preferred technical solution, the shielding protection in step 3 uses industrial tape and aluminum foil adhesive to isolate the part 1 from the tank liquid by laminating, smearing and adhering.
[0011] The beneficial effects of the present invention are: 1) By processing the reserved surface to leave a margin, even if there is an error in the thickness of the oxide layer, it can be removed in the secondary processing without any residue. There is no need to mask the conductive surface, which reduces the workload of workers and solves the problem of leakage of plating or masking deviation on the conductive surface; 2) The distance between the reserved surface and the conductive surface is 0.05mm, that is, a 0.05mm margin is left for the conductive surface during processing. If the margin is greater than 0.05mm, it will affect the processing time. If the margin is less than 0.05mm, the processing will be difficult and the processing accuracy will be easily affected. 3) Clean the surface of parts to improve the surface quality; 4) The masking protection in step 3 generally uses industrial tape and aluminum foil to isolate the parts and the tank liquid by laminating, smearing, and adhering. After the masking is completed, peeling will produce residual glue, which is removed by grinding; 5) If the current density is less than 2A / dm², the oxide layer will form slowly. If the current density is greater than 5A / dm², the uniformity and density of the oxide layer will be poor. BRIEF DESCRIPTION OF THE DRAWINGS
[0012] Figure 1 is a three-dimensional diagram of a part provided by one embodiment of the present invention; Figure 2 It is a three-dimensional diagram of a part of the structure provided by an embodiment of the present invention; Figure 3 is a cross-sectional view of a part provided by one embodiment of the present invention; exist Figure 1-Figure 3 In the formula, 1, parts; 101, conductive surface. DETAILED DESCRIPTION
[0013] The present invention is further described below in conjunction with the accompanying drawings.
[0014] The same or similar numbers in the drawings of the embodiments of the present invention correspond to the same or similar parts; in the description of the present invention, it should be understood that if the terms "head", "tail", "top", "bottom", "left", "right", "front", "back", "inside", "outside", etc. appear, the orientation or position relationship indicated is based on the orientation or position relationship shown in the drawings, which is only for the convenience of describing the present invention, and does not indicate or imply that the device or element referred to must have a specific orientation, be constructed and operate in a specific orientation. Therefore, the terms describing the position relationship in the drawings are only used for illustrative purposes and cannot be understood as a limitation on this patent. For ordinary technicians in this field, the specific meanings of the above terms can be understood according to specific circumstances.
[0015] See also Figure 1-Figure 3 One embodiment of the present invention provides a method for processing a local conductive position of an oxidized component, comprising the following steps: Step 1, drilling the part 1 to obtain a reserved surface, that is, leaving a processing allowance for the conductive surface 101; Step 2, oxidizing the part 1 obtained in step 1; Step 3, shielding and protecting the bottom surface of the component 1 obtained in step 2, removing the reserved surface obtained in step 2 and the oxide layer on the reserved surface, and obtaining the conductive surface 101; Step 4: clean the surface of the part 1 obtained in step 3.
[0016] By processing the reserved surface to leave a margin, even if there is an error in the thickness of the oxide layer, it can be removed in the secondary processing without any residue. There is no need to mask the conductive surface 101, which reduces the workload of workers and solves the problem of missing plating or masking offset of the conductive surface 101.
[0017] like Figure 1-Figure 3 As shown, the oxidation in step 2 is specifically hard anodizing, the bath liquid of the oxidation tank is sulfuric acid solution and sulfuric acid added with organic acid, such as oxalic acid and aminosulfonic acid, the bath liquid concentration is 10% to 30%, and the current density is 2-5A / dm². If the current density is less than 2A / dm², the oxide layer will be generated slowly. If the current density is greater than 5A / dm², the uniformity and density of the oxide layer will be poor.
[0018] like Figure 1-Figure 3 As shown, the distance between the reserved surface and the conductive surface 101 is 0.05mm, that is, the processing allowance is 0.05mm. The distance between the reserved surface and the conductive surface 101 is 0.05mm, that is, a 0.05mm allowance is left for the conductive surface 101 during processing. If the allowance is greater than 0.05mm, the processing time is affected. If the allowance is less than 0.05mm, the processing difficulty is great and the processing accuracy is easily affected.
[0019] like Figure 1-Figure 3As shown, the specific steps of step 4 are: grinding to remove the masking residual glue remaining on the surface of part 1, degreasing and cleaning to remove the oily cutting fluid remaining on the surface of part 1, and cleaning the surface of part 1 to improve the surface quality. The masking protection in step 3 generally uses industrial tape and aluminum foil glue to isolate part 1 and the tank liquid by fitting, smearing, and adhering. After the masking is completed, peeling will produce residual glue, which is removed by grinding.
[0020] The above embodiments are merely descriptions for the purpose of clearly illustrating the present invention, and are not limitations on the implementation methods. For technicians in the relevant field, other different forms of changes or modifications can be made based on the above descriptions. It is not necessary and impossible to list all the implementation methods here, and the obvious changes or modifications derived therefrom are still within the scope of protection of the present invention.
Claims
1. A method for processing the local conductive position of an oxidized part, Features , including the following steps: Step 1: Drill the parts to obtain a reserved surface; Step 2, oxidizing the parts obtained in step 1; Step 3, shielding and protecting the bottom surface of the component obtained in step 2, removing the reserved surface obtained in step 2 and the oxide layer on the reserved surface, and obtaining a conductive surface; Step 4: clean the surface of the parts obtained in step 3.
2. The method for processing the local conductive position of an oxidized component according to claim 1, It is characterized in that The distance between the reserved surface and the conducting surface is 0.05 mm.
3. The method for processing the local conductive position of an oxidized component according to claim 1, It is characterized in that The specific steps of step 4 are: grinding to remove the masking residual glue remaining on the surface of the part, and degreasing and cleaning to remove the oily cutting fluid remaining on the surface of the part.
4. The method for processing the local conductive position of an oxidized component according to claim 1, It is characterized in that The oxidation in step 2 is specifically hard anodizing, and the bath liquid of the oxidation tank is sulfuric acid solution or sulfuric acid with organic acid added.
5. The method for processing the local conductive position of an oxidized component according to claim 4, It is characterized in that The organic acid is oxalic acid or aminosulfonic acid.
6. The method for processing the local conductive position of an oxidized component according to claim 4, It is characterized in that The current density during oxidation in step 2 is 2-5A / dm².
7. The method for processing the local conductive position of an oxidized component according to claim 1, It is characterized in that The masking protection in step 3 uses industrial tape and aluminum foil adhesive to isolate part 1 from the tank liquid by laminating, smearing and adhering.
Citation Information
Patent Citations
Technique for controlling precision hole anode oxidization process for L6 aluminum alloy part
CN106381515A
Method for processing high-precision stainless steel parts
CN107052712A
Anodic oxidation method
CN110257877A
ABS / ESC valve body machining method for automobile braking system
CN111112943A
Method for treating surface of metal using anodizing process
KR1020130078148A