Laser welding method for controlling crankshaft welding deformation

Through laser welding method, spot welding is first performed and positioned and then horizontal welding gaps are welded, the welding sequence and rotation speed are adjusted, which solves the problem of welding deformation control of the ring weld seam of the small circular tube ribbed structure, improves the welding quality and accuracy, and is suitable for automobile manufacturing. crankshaft parts.

CN118989595AActive Publication Date: 2024-11-22ZHENJIANG XIANFENG AUTOMOBILE COMPONENTS CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411415518.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-11
Publication Date
2024-11-22
Estimated Expiration
2044-10-11

AI Technical Summary

Technical Problem

The prior art is difficult to effectively control the welding deformation of the annular weld of the small round tube ribbed structure, especially in the welding process of crankshaft parts in automobile manufacturing, the welding deformation control method is insufficient, which affects the welding quality and accuracy.

Method used

Using laser welding method, first place the spindle vertically for spot welding and positioning, then place horizontally for annular gap welding. By adjusting the welding sequence and rotation speed, welding deformation is controlled. The laser welding device includes a processing platform, a laser lens module, and three Coordinate moving components, top-end, rotating components and positioning components to ensure welding accuracy and quality.

Benefits of technology

It improves the quality and processing accuracy of welds, reduces the number of clamping times, and avoids welding quality problems. It is suitable for ring welds in small round tube rib structures, controls the overall deformation of the spindle, and controls the cylindrical error within 0.1mm.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989595A_ABST
    Figure CN118989595A_ABST
Patent Text Reader

Abstract

The invention provides a laser welding method for controlling crankshaft welding deformation. The laser welding method comprises the following steps that 10, a main shaft is vertically placed, a crank is installed on the main shaft according to a forming scheme, the main shaft and the crank are fixed, and laser spot welding positioning is conducted on an annular gap between the crank and the main shaft; and step 20, horizontally placing the main shaft, fixing the main shaft, and carrying out laser welding on an annular gap between the crank and the main shaft to obtain the crankshaft. The invention provides a laser welding method for controlling crankshaft welding deformation. The welding seam quality and the machining precision can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of laser welding, and in particular relates to a laser welding method for controlling crankshaft welding deformation. Background Art

[0002] Laser welding is a high-quality welding method characterized by high precision and excellent controllability. Its high energy density and localized heat input enable the production of small welds with controllable penetration depth and width. Furthermore, the heat-affected zone (HAZ) is very narrow, making it easy to control weld size and position at the micron level. Laser welding offers high speed, high efficiency, and ease of automation. In recent years, it has been widely used in various industries, including automotive, aerospace, electronics, and medical devices.

[0003] The crankshaft is a slender, circular tube-ribbed structure consisting of a main shaft and a crank. The crank is mounted on the main shaft, which is a slender circular tube, and the crank is a ribbed plate. As a critical component in automotive manufacturing, it performs crucial functions such as transmitting torque, converting motion (converting reciprocating linear motion to rotational motion, and vice versa), and connecting components. During use, it must withstand certain axial and radial loads, placing high demands on the crankshaft's manufacturing precision, assembly accuracy, component performance, and structural performance. For slender, circular tube-ribbed structures like crankshafts, laser welding to connect the crank to the main shaft is the most economical and reliable manufacturing method.

[0004] Extensive research on girth welds in circular tube-ribbed structures has focused primarily on controlling the weld deformation of large pipelines, such as wind turbine jacket steel tubes and underground transmission pipelines. This research focuses on performance issues such as coarse weld microstructure and softening in the heat-affected zone (HAZ). However, limited research exists on methods for controlling the weld deformation of girth welds in small circular tubes (diameter ≤ 40 mm). Currently, there are methods for controlling deformation in thick-walled circular tubes and thin-walled stainless steel pressure vessels by controlling the welding sequence of the groove welds. Specialized tooling has also been designed to control weld deformation, but these methods are limited in scope and are not suitable for controlling the weld deformation of circular tube girth welds, particularly those with diameters between 60 and 200 mm and wall thicknesses ≤ 2 mm. Therefore, to address the development of the automotive industry and to address the gap in weld deformation control for girth welds in slender circular tube-ribbed structures, it is necessary to develop a laser welding device and overall weld deformation control process suitable for small circular tube-ribbed structures. Summary of the Invention

[0005] The technical problem to be solved by the present invention is to provide a laser welding method for controlling the welding deformation of a crankshaft, thereby improving the weld quality and processing accuracy.

[0006] To solve the above technical problems, an embodiment of the present invention provides a laser welding method for controlling crankshaft welding deformation, comprising the following steps: Step 10: Place the main shaft vertically, install the crank onto the main shaft according to the molding plan, fix the main shaft and crank, and perform laser spot welding on the annular gap between the crank and the main shaft; Step 20: Place the main shaft horizontally, fix the main shaft, and laser weld the annular gap between the crank and the main shaft to obtain the crankshaft.

[0007] As a further improvement to the embodiment of the present invention, the diameter of the main shaft is less than or equal to 40 mm, the length of the main shaft is 100-400 mm, and the number of cranks is 3-12.

[0008] As a further improvement to the embodiment of the present invention, in step 20, if there are 2N+1 cranks, the annular gap between the N+1th crank and the main shaft is first welded; then the Nth and 2N+1th cranks are grouped together, and the annular gaps between them and the main shaft are welded respectively; then the N+2th and 1st cranks are grouped together, and the annular gaps between them and the main shaft are welded respectively; in this way, the crank closest to the N+1th crank and the crank closest to the edge are grouped together, and the annular gaps between them and the main shaft are welded respectively, until the annular gaps between all cranks and the main shaft are welded; in each group of cranks, the two cranks are located on either side of the centerline of the main shaft; If there are 2N cranks, first group the Nth and N+1th cranks together, and weld the annular welds between them and the main shaft respectively; then group the N-1th and 2Nth cranks together, and weld the annular gaps between them and the main shaft respectively; then group the N+2th and 1st cranks together, and weld the annular gaps between them and the main shaft respectively; in turn, group the crank closest to the Nth or N+1th crank and the crank closest to the edge together, and weld the annular gaps between them and the main shaft respectively, until the annular gaps between all cranks and the main shaft are welded; in each group of cranks, the two cranks are located on either side of the centerline of the main shaft; where N is an integer greater than or equal to 1.

[0009] As a further improvement of the embodiment of the present invention, the number of cranks is 3, which are the first crank, the second crank and the third crank in the axial direction of the main shaft; In step 20, after the main shaft is fixed, the annular gap between the second crank and the main shaft is first welded, then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the third crank and the main shaft is laser welded.

[0010] As a further improvement of the embodiment of the present invention, the number of cranks is 4, which are the first crank, the second crank, the third crank and the fourth crank in order along the axial direction of the main shaft; In step 20, after fixing the main shaft, the annular gap between the second crank and the main shaft is first welded, then the annular gap between the third crank and the main shaft is laser welded, then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the fourth crank and the main shaft is laser welded.

[0011] As a further improvement of the embodiment of the present invention, the number of cranks is 5, which are the first crank, the second crank, the third crank, the fourth crank and the fifth crank in the axial direction of the main shaft; In step 20, after fixing the main shaft, the annular gap between the third crank and the main shaft is first welded, and then the annular gap between the second crank and the main shaft is laser welded, and then the annular gap between the fifth crank and the main shaft is laser welded, and then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the fourth crank and the main shaft is laser welded.

[0012] As a further improvement of the embodiment of the present invention, in steps 10 and 20, during laser welding, the distance between the welding head and the annular gap between the crank and the main shaft is 3 to 10 mm, and the angle between the welding head and the vertical plane is 15° to 60°.

[0013] As a further improvement to the embodiment of the present invention, in step 20, when laser welding is performed on the annular gap between the same crank and the main shaft, the welding head does not move, and the rotation speed is obtained according to the diameter of the annular gap, driving the main shaft to rotate at the rotation speed.

[0014] As a further improvement of the embodiment of the present invention, the rotation speed is calculated according to the diameter of the annular gap using formula (1): ω=60v / (π×d) Formula (1) Wherein, ω represents the rotation speed, the unit is r / min; v represents the welding speed, the unit is mm / s; d represents the diameter of the annular weld, the unit is mm.

[0015] As a further improvement to an embodiment of the present invention, a laser welding device is used; the laser welding device includes a processing platform, a laser lens module, a three-coordinate moving assembly, a center, a rotating assembly and a positioning assembly; the laser lens module is mounted on the processing platform via the three-coordinate moving assembly; the three-coordinate moving assembly is used to drive the laser lens module to move three-dimensionally relative to the processing platform; the center and the rotating assembly are relatively arranged on the processing platform, and the rotating assembly is used to drive the spindle to rotate; the positioning assembly is mounted on the processing platform, and is used to fix the spindle and crank before spot welding positioning, and to transport the spindle together with the crank to between the center and the rotating assembly after the spot welding positioning is completed.

[0016] Compared with the prior art, the technical solution of the present invention has the following beneficial effects: (1) The method of the present invention first places the main shaft vertically, installs the crank onto the main shaft, and spot welds the crank. The crank can be positioned on the main shaft after spot welding, and there is no need to clamp and fix the crank. Moreover, spot welding is only performed on one side, and no overhead welding will occur. Then the main shaft is placed horizontally, and only the main shaft needs to be fixed. The annular gap between the crank and the main shaft is welded in turn. Regardless of whether single-side welding or double-side welding is performed, overhead welding will not occur, which will cause the quality of the weld to deteriorate. The method of the present invention first performs vertical spot welding positioning, and then horizontally welds the gap. The process is simple, reduces the number of clamping times, improves the quality of the weld, improves the processing accuracy, avoids the welding quality problems that may be caused by selecting different welding methods, and better guarantees the overall welding quality of the parts. The method of the present invention adopts laser welding, and the diameter of the laser spot can generally be controlled between 0.5mm and 2mm, which meets the requirements of small annular weld gap width and high precision of small circular tube rib plate structures; and when horizontally welding the gap, a four-jaw self-centering chuck is used to fix a circular tubular spindle with a smaller diameter, which is firmly fixed and easy to clamp, and is suitable for welding annular welds of small circular tube rib plate structures.

[0017] (2) The method of the present invention takes into account the multiple small welding deformations that will occur when welding different cranks. By adjusting the welding sequence of the cranks according to their positional relationship on the spindle, the welding stresses generated in multiple locations can be offset (checked and balanced) against each other, thereby achieving mutual regulation of welding deformations and achieving the purpose of controlling the total deformation of the spindle. Even if the spindle has a small diameter, a long length, and a large number of cranks, the cylindricity error of the spindle axis deformation can be controlled within 0.1 mm. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Figure 1 This is a flow chart of a laser welding method for controlling crankshaft welding deformation according to an embodiment of the present invention; Figure 2 Schematic diagram of the structure of a feeding device of a laser welding device used in a laser welding method according to an embodiment of the present invention; Figure 3 A structural diagram of a crankshaft.

[0019] The figure includes: processing platform 1, laser lens module 2, three-coordinate moving assembly 3, top 4, base 51, four-jaw self-centering chuck 52, positioning tooling 61, lifting assembly 62, rotating assembly 63, crankshaft 7, main shaft 71, crank 72, first annular gap 73, second annular gap 74, third annular gap 75, laser water cooling box 8, laser generator 9, and controller 10. DETAILED DESCRIPTION

[0020] The technical solution of the present invention is described in detail below with reference to the accompanying drawings.

[0021] The embodiment of the present invention provides a laser welding method for controlling crankshaft welding deformation, such as Figure 1 As shown, the following steps are included: Step 10: Place the main shaft vertically, install the crank onto the main shaft according to the molding plan, fix the main shaft and the crank, and perform laser spot welding on the annular gap between the crank and the main shaft.

[0022] The diameter of the main shaft is less than or equal to 40 mm, the length of the main shaft is 100 to 400 mm, and the number of cranks is 3 to 12.

[0023] Preferably, a three-point positioning spot welding method can be adopted, and the three welding points are evenly distributed on the annular gap.

[0024] Step 20: Place the main shaft horizontally, fix the main shaft, and laser weld the annular gap between the crank and the main shaft to obtain the crankshaft.

[0025] Preferably, in steps 10 and 20, during welding, the distance between the welding head and the annular gap between the crank and the main shaft is 3 to 10 mm, and the angle between the welding head and the vertical plane is 15° to 60°. During laser welding, changes in welding height will change the defocus of the laser, that is, the distance between the laser focal plane and the welding surface. The distance between the welding head and the annular gap is 3 to 10 mm, which can obtain a suitable defocus, effectively improving the welding quality. The angle between the welding head and the vertical plane is 15° to 60°, which prevents high-energy laser light from being reflected back to the lens group and damaging the lens assembly, while ensuring that the laser energy is effectively absorbed, thereby improving the welding quality.

[0026] Preferably, in step 20, if there are 2N+1 cranks, the annular gap between the N+1th crank and the main shaft is welded first; then the Nth and 2N+1th cranks are grouped together, and the annular gaps between them and the main shaft are welded separately; then the N+2th and 1st cranks are grouped together, and the annular gaps between them and the main shaft are welded separately; and the crank closest to the N+1th crank and the crank closest to the edge are grouped together, and the annular gaps between them and the main shaft are welded separately, until the annular gaps between all cranks and the main shaft are welded. In each group of cranks, the two cranks are located on either side of the centerline of the main shaft. In each group of cranks, there is no restriction on the order in which the annular gaps between the two cranks and the main shaft are welded.

[0027] If there are 2N cranks, first group the Nth and N+1th cranks together, and weld the annular welds between them and the spindle. Then, group the N-1th and 2Nth cranks together, and weld the annular gaps between them and the spindle. Next, group the N+2th and 1st cranks together, and weld the annular gaps between them and the spindle. Sequentially group the crank closest to the Nth or N+1th crank and the crank closest to the edge together, and weld the annular gaps between them and the spindle, respectively. This process continues until all the annular gaps between the cranks and the spindle are welded. (N is an integer greater than or equal to 1.) In each group of cranks, the two cranks are located on either side of the centerline of the spindle. Within each group, there is no restriction on the order in which the annular gaps between the two cranks and the spindle are welded.

[0028] During welding using the method of this embodiment, the welding sequence is determined by the number of cranks. If the number of cranks is odd, start with the center crank; if the number of cranks is even, start with the two center cranks. When welding the remaining cranks, span welding is performed, meaning the cranks near the center and those near the edges are welded in pairs. This effectively prevents heat buildup while controlling deformation and welding stress.

[0029] For example, the number of cranks is 3. After spot welding, Figure 3 As shown, three cranks 72 are arranged axially along the main shaft 71, namely the first crank, the second crank, and the third crank. The annular gaps between the first crank, the second crank, and the third crank and the main shaft are respectively the first annular gap 73, the second annular gap 74, and the third annular gap 75. In step 20, after the main shaft is fixed, the second annular gap 74 between the second crank and the main shaft is first welded, then the first annular gap 73 between the first crank and the main shaft is welded, and finally the third annular gap 75 between the third crank and the main shaft is welded.

[0030] There are four cranks. After spot welding, the four cranks 72 are arranged axially along the main shaft 71, in the order of the first crank, the second crank, the third crank, and the fourth crank. In step 20, after the main shaft is fixed, the annular gap between the second crank and the main shaft is first welded, then the annular gap between the third crank and the main shaft is laser welded, then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the fourth crank and the main shaft is laser welded.

[0031] There are five cranks. After spot welding, the five cranks are arranged along the main shaft axis, in the order of the first crank, the second crank, the third crank, the fourth crank, and the fifth crank. In step 20, after the main shaft is fixed, the annular gap between the third crank and the main shaft is first welded, followed by laser welding the annular gap between the second crank and the main shaft, then laser welding the annular gap between the fifth crank and the main shaft, then laser welding the annular gap between the first crank and the main shaft, and finally laser welding the annular gap between the fourth crank and the main shaft.

[0032] Preferably, in step 20, when laser welding the annular gap between the same crank and the main shaft, the welding head does not move, a suitable welding speed is set, and the rotation speed of the main shaft is determined according to the diameter of the annular gap, and the main shaft rotates with the crank at this rotation speed.

[0033] Specifically, the spindle rotation speed is calculated using formula (1): ω=60v / (π×d) Formula (1) Where ω represents the spindle rotation speed in r / min; v represents the welding speed in mm / s; d represents the annular weld diameter in mm.

[0034] Five specific examples are provided below.

[0035] Example 1 The main shaft has a diameter of 40 mm and a length of 100 mm, and three cranks are welded thereon. The first crank, the second crank, and the third crank are sequentially arranged on the main shaft.

[0036] After spot welding, the annular gaps between the three cranks and the spindle were welded in the following order: second crank, first crank, third crank. During welding, the welding head was 5 mm from the annular gap between the cranks and the spindle, the angle between the welding head and the vertical plane was 30°, the welding speed was 10 mm / s, and the spindle rotation speed was 5 rpm.

[0037] After getting the crankshaft, use the radius measurement method [1] The measured cylindricity error of the spindle axis deformation is 0.05mm.

[0038] Example 2 The main shaft has a diameter of 40 mm and a length of 150 mm, and four cranks are welded thereon. The first crank, the second crank, the third crank, and the fourth crank are sequentially arranged on the main shaft.

[0039] After spot welding, the annular gaps between the four cranks and the spindle were welded in the following order: second crank, third crank, first crank, and fourth crank. During welding, the weld head was 5 mm from the annular gap between the cranks and the spindle, the angle between the weld head and the vertical plane was 30°, the welding speed was 10 mm / s, and the spindle rotation speed was 5 rpm.

[0040] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.05mm.

[0041] Example 3 The main shaft has a diameter of 40 mm and a length of 200 mm, and five cranks are welded thereon. The first crank, the second crank, the third crank, the fourth crank, and the fifth crank are sequentially arranged on the main shaft.

[0042] After spot welding, the order of welding the annular gaps between the five cranks and the spindle was as follows: crank 3, crank 2, crank 5, crank 1, crank 4. During welding, the distance between the welding head and the annular gap between the cranks and the spindle was 5 mm, the angle between the welding head and the vertical plane was 30°, the welding speed was 10 mm / s, and the spindle rotation speed was 5 rpm.

[0043] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.08mm.

[0044] Example 4 The main shaft has a diameter of 40 mm and a length of 400 mm, and 11 cranks are welded thereon. The first crank, the second crank, the third crank, the fourth crank, the fifth crank, the sixth crank, the seventh crank, the eighth crank, the ninth crank, the tenth crank, and the eleventh crank are sequentially arranged on the main shaft.

[0045] After spot welding, the order of welding the annular gaps between the 11 cranks and the spindle was as follows: crank 6, crank 5, crank 11, crank 7, crank 1, crank 2, crank 8, crank 4, crank 10, crank 3, crank 9. During welding, the distance between the welding head and the annular gap between the cranks and the spindle was 5 mm, the angle between the welding head and the vertical plane was 30 degrees, the welding speed was 10 mm / s, and the spindle rotation speed was 5 rpm.

[0046] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.1mm.

[0047] Example 5 The main shaft has a diameter of 40 mm and a length of 450 mm, and is welded with 12 cranks. The first crank, the second crank, the third crank, the fourth crank, the fifth crank, the sixth crank, the seventh crank, the eighth crank, the ninth crank, the tenth crank, the eleventh crank, and the twelfth crank are sequentially arranged on the main shaft.

[0048] After spot welding, the order of welding the annular gaps between the 12 cranks and the spindle was as follows: crank 6, crank 7, crank 5, crank 12, crank 1, crank 8, crank 4, crank 11, crank 9, crank 2, crank 3, crank 10. During welding, the distance between the welding head and the annular gap between the cranks and the spindle was 5 mm, the angle between the welding head and the vertical plane was 30 degrees, the welding speed was 10 mm / s, and the spindle rotation speed was 5 rpm.

[0049] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.1mm.

[0050] Comparative Example 1 The same as Example 1, except that the order of welding the annular gaps between the three cranks and the main shaft is: the first crank, the second crank, and the third crank.

[0051] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.1 mm.

[0052] Comparative Example 2 The same as Example 2, except that the order of welding the annular gaps between the four cranks and the main shaft is: the first crank, the second crank, the third crank, and the fourth crank.

[0053] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.2 mm.

[0054] Comparative Example 3 The same as Example 3, except that the order of welding the annular gaps between the five cranks and the main shaft is: the first crank, the second crank, the third crank, the fourth crank, and the fifth crank.

[0055] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 0.5 mm.

[0056] Comparative Example 4 The same as Example 4, except that the order of welding the annular gaps between the 11 cranks and the main shaft is: the first crank, the second crank, the third crank, the fourth crank, the fifth crank, the sixth crank, the seventh crank, the eighth crank, the ninth crank, the tenth crank, and the eleventh crank.

[0057] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 3 mm.

[0058] Comparative Example 5 The same as Example 5, except that the order of welding the annular gaps between the 12 cranks and the main shaft is: the first crank, the second crank, the third crank, the fourth crank, the fifth crank, the sixth crank, the seventh crank, the eighth crank, the ninth crank, the tenth crank, the eleventh crank, and the twelfth crank.

[0059] After obtaining the crankshaft, the radius measurement method was used to measure the axis deformation cylindricity error of the main shaft, which was 3.5 mm.

[0060] It can be seen from the above five examples and five comparative examples that the welding sequence of the present invention can significantly reduce the axis deformation and cylindricity error of the main shaft and improve product precision.

[0061] The embodiment method of the present invention adopts Figure 2 The laser welding device shown. The laser welding device includes a processing platform 1, a laser lens module 2, a three-coordinate moving assembly 3, a centering tip 4, a rotating assembly, and a positioning assembly. It also includes a laser water cooling box 8, a laser generator 9, and a controller 10. The laser water cooling box 8 and the laser generator 9 are both connected to the laser lens module 2, and the laser lens module 2, the three-coordinate moving assembly 3, the rotating assembly, and the positioning assembly are all connected to the controller 10. The laser lens module 2 is mounted on the processing platform 1 via the three-coordinate moving assembly 3, which is used to drive the laser lens module 2 to move three-dimensionally relative to the processing platform 1. The centering tip 4 and the rotating assembly are arranged relative to each other on the processing platform 1, and the rotating assembly is used to drive the spindle 71 to rotate. The rotating assembly includes a base 51, a four-jaw self-centering chuck 52, and a drive motor. The four-jaw self-centering chuck 52 and the drive motor are mounted on the base 51, with the four-jaw self-centering chuck 52 facing the centering tip 4. The drive motor is connected to the four-jaw self-centering chuck 52 to drive the four-jaw self-centering chuck 52 to rotate. The positioning assembly is mounted on the machining platform 1 and is used to secure the spindle 71 and crank 72 before spot welding. After spot welding, the spindle and crank are transferred between the center pin 4 and the rotating assembly. The positioning assembly comprises a positioning fixture 61, a lifting assembly 62, and a rotating assembly 63. The positioning fixture 61 is mounted on the lifting assembly 62 via the rotating assembly 63, and the lifting assembly 62 is mounted on the machining platform 1. The rotating assembly 63 drives the positioning fixture 61 to rotate, while the lifting assembly 62 drives the positioning fixture 61 up and down.

[0062] The method of the embodiment of the present invention uses the above-mentioned laser welding device, including the following steps: Step 10: Place the spindle vertically, install the crank onto the spindle according to the molding plan, and secure the spindle and crank using the positioning assembly. The three-dimensional motion assembly 3 drives the laser lens module 2 to move three-dimensionally relative to the machining platform 1, bringing the laser lens module 2 close to the spindle. The distance between the welding head and the annular gap between the crank and the spindle, as well as the angle between the welding head and the vertical plane, are adjusted. Spot welds are then performed on the annular gap between each crank and the spindle to ensure that each crank is positioned on the spindle.

[0063] In step 20, the main shaft and the crank are transported between the top 4 and the rotating assembly through the positioning assembly, the main shaft is placed horizontally, and the main shaft is fixed by the top 4 and the rotating assembly. The laser lens module 2 is driven by the three-dimensional moving assembly 3 to move three-dimensionally relative to the processing platform 1, so that the laser lens module 2 is close to the main shaft, and the distance between the welding head and the annular gap between the crank and the main shaft, as well as the angle between the welding head and the vertical plane are adjusted. According to the welding sequence, the annular gap between each crank and the main shaft is welded in turn. During the process of welding an annular gap, the three-dimensional moving assembly 3 does not drive the laser lens module 2 to move, but drives the main shaft to rotate through the rotating assembly.

[0064] The above description is only a specific embodiment of the present invention, but the scope of protection of the present invention is not limited thereto. Any changes or substitutions that can be easily conceived by any technician familiar with this technical field within the technical scope disclosed in the present invention should be covered by the scope of protection of the present invention.

[0065] [1] Chen Jianjun, Li Jun. Discussion on cylindricity error based on radius measurement method[J]. Science and Technology Information, 2017, 15(31):18-19.DOI:10.16661 / j.cnki.1672-3791.2017.31.018.

Claims

1. A laser welding method for controlling crankshaft welding deformation, characterized in that: The following steps are involved: Step 10, placing the main shaft vertically, installing the crank onto the main shaft according to the molding plan, fixing the main shaft and the crank, and performing laser spot welding positioning on the annular gap between the crank and the main shaft; Step 20, placing the main shaft horizontally, fixing the main shaft, and laser welding the annular gap between the crank and the main shaft to obtain the crankshaft.

2. The laser welding method for controlling crankshaft welding deformation according to claim 1, characterized in that: The diameter of the main shaft is less than or equal to 40 mm, the length of the main shaft is 100-400 mm, and the number of cranks is 3-12.

3. The laser welding method for controlling crankshaft welding deformation according to claim 1, characterized in that: In step 20, if there are 2N+1 cranks, first weld the annular gap between the N+1th crank and the main shaft; then take the Nth and 2N+1th cranks as a group, and weld the annular gaps between them and the main shaft respectively; then take the N+2th and 1st cranks as a group, and weld the annular gaps between them and the main shaft respectively; in this way, take the crank closest to the N+1th crank and the crank closest to the edge as a group, and weld the annular gaps between them and the main shaft respectively, until the annular gaps between all cranks and the main shaft are welded; in each group of cranks, two cranks are located on both sides of the center line of the main shaft respectively; If there are 2N cranks, first take the Nth and N+1th cranks as a group, and weld the annular welds between them and the main shaft respectively; then take the N-1th and 2Nth cranks as a group, and weld the annular gaps between them and the main shaft respectively; then take the N+2th and 1st cranks as a group, and weld the annular gaps between them and the main shaft; successively take the cranks closest to the Nth or N+1th crank and the crank closest to the edge as a group, and weld the annular gaps between them and the main shaft respectively, until the annular gaps between all cranks and the main shaft are welded; in each group of cranks, the two cranks are located on both sides of the centerline of the main shaft; wherein N represents an integer greater than or equal to 1.

4. The laser welding method for controlling crankshaft welding deformation according to claim 3, characterized in that: The number of cranks is 3, which are the first crank, the second crank and the third crank in order along the axis of the main shaft; In step 20, after the main shaft is fixed, the annular gap between the second crank and the main shaft is first welded, then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the third crank and the main shaft is laser welded.

5. The laser welding method for controlling crankshaft welding deformation according to claim 3, characterized in that: The number of cranks is 4, which are the first crank, the second crank, the third crank and the fourth crank in order along the axis of the main shaft; In step 20, after fixing the main shaft, the annular gap between the second crank and the main shaft is first welded, then the annular gap between the third crank and the main shaft is laser welded, then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the fourth crank and the main shaft is laser welded.

6. The laser welding method for controlling crankshaft welding deformation according to claim 3, characterized in that: The number of cranks is 5, which are the first crank, the second crank, the third crank, the fourth crank and the fifth crank in order along the axis of the main shaft; In step 20, after fixing the main shaft, the annular gap between the third crank and the main shaft is welded first, and then the annular gap between the second crank and the main shaft is laser welded, and then the annular gap between the fifth crank and the main shaft is laser welded, and then the annular gap between the first crank and the main shaft is laser welded, and finally the annular gap between the fourth crank and the main shaft is laser welded.

7. The laser welding method for controlling crankshaft welding deformation according to claim 1, characterized in that: In step 10 and step 20, during laser welding, the distance between the welding head and the annular gap between the crank and the main shaft is 3 to 10 mm, and the angle between the welding head and the vertical plane is 15° to 60°.

8. The laser welding method for controlling crankshaft welding deformation according to claim 1, characterized in that: In step 20, when laser welding is performed on the annular gap between the same crank and the main shaft, the welding head does not move, and the main shaft and the crank rotate synchronously.

9. The laser welding method for controlling crankshaft welding deformation according to claim 8, characterized in that: According to the annular gap diameter, the spindle rotation speed is calculated using formula (1): ω=60v / (π×d) Formula (1) Wherein, ω represents the spindle rotation speed, the unit is r / min; v represents the welding speed, the unit is mm / s; d represents the annular weld diameter, the unit is mm.

10. The laser welding method for controlling crankshaft welding deformation according to claim 1, characterized in that: A laser welding device is used; the laser welding device includes a processing platform, a laser lens module, a three-coordinate moving component, a center, a rotating component and a positioning component. The laser lens module is installed on the processing platform through the three-coordinate moving component, and the three-coordinate moving component is used to drive the laser lens module to move three-dimensionally relative to the processing platform; the center and the rotating component are relatively arranged on the processing platform, and the rotating component is used to drive the main shaft to rotate; the positioning component is installed on the processing platform, and is used to fix the main shaft and the crank before spot welding positioning, and transport the main shaft and the crank between the center and the rotating component after the spot welding positioning is completed.

Citation Information

Patent Citations

  • Laser welding method of turbine disc and rotating shaft

    CN101480760A

  • Flange welding process by rotating main shaft for 90 degrees

    CN110449695A

  • Welding detection device for driving shaft and welding detection method

    CN113510399A

  • Laser hardening method of crank shaft

    JP2016176542A