Combination manufacturing method for aluminum alloy three-way half-pipe parts with complex molded surfaces and convex edge holes

By adopting the process of cutting of deep drawing forming, drilling, stamping convex edges and laser cutting machines, problems such as large changes in the shape of the corners and limited flow of sheets during the forming of aluminum alloy tee half-pipe parts are solved, and the problem of large changes in the shape of the shape surface and limited flow of sheets is achieved. The surface quality of parts and the production efficiency are improved, and the scrap rate is significantly reduced.

CN118989876APending Publication Date: 2024-11-22SHENYANG AIRCRAFT CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411217712.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-02
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

In the prior art, during the forming process of aluminum alloy tee half-pipe parts, there are large changes in the curvature of the shape at corners, limited flow of sheets, easy cracking by hand forming, severe edge folds, many surface hammer marks, insufficient tire degree, The problems of small thickness difficult to meet, difficult manual cutting operation, low efficiency and high scrap rate.

Method used

Using the process of cutting shapes of drawing, drilling, stamping convex edges and laser cutting machines, replacing the traditional manual forming and manual shearing methods, using special drawing dies, drilled-cover mold tires, convex edge dies and lasers Cutting fixtures are processed.

Benefits of technology

The surface quality of the parts is improved, cracking and wrinkling problems are reduced, labor intensity is reduced, production cycle is shortened, dimensional accuracy and tire degree are improved, and the scrap rate is reduced from 70% to 10%.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118989876A_ABST
    Figure CN118989876A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of aviation aircraft aluminum alloy sheet metal machining, and relates to a combined manufacturing method for aluminum alloy three-way half-pipe parts with complex molded surfaces and convex edge holes. After the aluminum alloy three-way half-pipe part with the complex molded surface and the convex edge hole is formed through the novel combined manufacturing method, the problems of cracking, wrinkling, not-in-place forming and multiple surface hammer marks caused by manual forming are solved, the problems of high labor intensity and out-of-tolerance size caused by manual shape shearing are solved, the surface quality of the part is improved, and the production cost is reduced. And the surface roughness is improved to be not greater than Ra3.2 microns. According to the part formed through the method, the tire attaching degree is smaller than 0.5 mm, the shape limit deviation meets + / -0.5 mm, the production period for machining the aluminum alloy three-way half-pipe part with the complex profile is shortened to 2 hours from 6-8 hours, and the rejection rate is reduced to 10% from 70%.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of aluminum alloy sheet metal processing for aviation aircraft, and relates to a method for manufacturing an aluminum alloy three-way half-tube component assembly with a complex profile and convex edge holes. Background Art

[0002] The aluminum alloy three-way half-pipe part is a power oil conduit part, installed in the rear compartment of the fuel tank. As a connecting pipe, it has a complex curved surface and a convex hole structure. Due to the complex surface structure of half-pipe parts and the irregular flow of sheet metal during the forming process, it is impossible to give an accurate unfolded material size. The only way is to use the rough material to form the outer edge of the part according to the edge line of the tooling. The typical process flow is "straight line cutting - manual forming - manual cutting shape". The part described in the present invention is made of 2.5mm thick rust-proof aluminum sheet, and its shape is as follows: Figure 1 As shown in the figure, the typical processing method is: the shearing machine shears the square aluminum alloy sheet, the sheet is manually sheared into the initial shape, the part surface is manually formed using a mold, and then the bottom hole is opened through the mold and the convex hole is manually formed with the help of the core, and the edge contour of the part is manually marked with a stylus according to the matching mold, and the irregular contour is cut according to the marking line using a high-speed band saw combined with the manual shearing method, and the edge protrusions and burrs are filed and trimmed to meet the shape limit deviation of ±0.5mm. Due to the complex structure of the parts, the following problems exist in production: ① The curvature of the surface at the corner of the three-way half-tube part changes greatly, the flow of the sheet is limited, the hand-formed corner is prone to cracking, the scrap rate is high, and the corner edge is severely wrinkled, and there are many hammer marks on the surface. After subsequent sandpaper polishing, it is difficult to meet the requirement that the surface roughness of the part is not greater than Ra3.2μm. ② Due to the thickness of the sheet, when the convex hole on the curved surface of the three-way half-tube is manually formed, the forming is not in place, and the degree of adhesion is difficult to meet the requirement of less than 0.5mm. ③ After the edge of the part is manually marked, the band saw cutting combined with manual shearing of the 2.5mm thick aluminum alloy part is difficult to operate, labor-intensive, and inefficient. The dimensional accuracy of the part cannot be guaranteed and is prone to over-tolerance. In summary, using traditional processing methods, the scrap rate of parts is as high as 70%, the total processing time for one piece is 6 to 8 hours, the production efficiency is low, and the quality of parts needs to be improved. Summary of the invention

[0003] The purpose of the present invention is to invent a method for manufacturing an aluminum alloy three-way and half-tube sheet metal parts assembly. The manufacturing method optimizes the parts processing process method, replaces manual forming with mechanical forming, and applies laser cutting technology, using the process flow of "deep drawing-drilling-stamping convex edge-laser cutting machine cutting shape" to replace the traditional process flow of "manual forming-drilling-manual shearing shape".

[0004] A special drawing die is used for deep drawing, a special die with a drill sleeve is used for drilling, a special convex die is used for stamping convex edges, and a special laser cutting fixture is used for cutting the shape by a laser cutting machine. The first step is to draw the overall surface of the part; the second step is to use the drill sleeve on the special die to drill a 1-φ5.2mm hole in the center of the convex hole, and expand the hole to a 1-φ10mm through hole; the third step is to use a special convex die to stamp and form the convex hole on the half-tube curved surface; the fourth step is to use a laser cutting machine to cut the theoretical shape contour around the part to make the part meet the qualified requirements.

[0005] In order to achieve the above object, the technical solution of the present invention is:

[0006] The first step: deep drawing. The tooling used in the deep drawing process is the "drawing die", which includes: upper template, concave die, blank holder, punch, lower template, guide pin, guide sleeve, unloading screw, lifting ring, die handle fixing screw, cylindrical pin, fixing screw, die handle.

[0007] The tooling "drawing die" can realize the deep drawing of aluminum alloy sheets. The upper and lower templates are made of Q235-AF steel; the concave die, blank holder and punch are made of Cr12MoV steel, which are heat treated to a hardness of 59-62HRC. The gap between the concave die and the punch is 1.1 times the material thickness. The manufacturing tolerance of the "drawing die" tooling surface is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm. The punch and the lower template of the "drawing die" tooling are connected and fixed by hole matching, and the concave die and the upper template are connected and fixed by hole matching. The unloading screw and the blank holder form a pusher, which always pushes the formed parts up to play a role in unloading. The two guide sleeves installed on the upper template and the two guide pillars installed on the lower template adopt H5 / h5 clearance matching, and the two guide pillars play a limiting role. Before deep drawing, the blank holder is pushed up by the unloading screw to keep it away from the lower template and placed above the punch. The distance between the blank holder and the lower template is greater than the part profile height. The part blank is placed on the blank holder and lubricating oil is evenly applied to the front and back sides of the part blank along the theoretical shape.

[0008] When the "drawing die" is working, the stamping hydraulic press moves downward, and the die handle drives the upper die plate and the die to move downward together, and the die begins to close. The die continues to move downward until it fits with the blank holder ring and drives the blank holder ring to move downward together. The sheet metal contacts the punch, and the part begins to form. The upper die plate, the die, the blank holder ring, the punch, and the lower die plate slide with the guide sleeve and the guide column. The sheet metal is pushed up by the punch into the groove of the die until the blank holder ring moves down to the lower die plate, and the closing of the die is completed. When the mold is opened, the die moves upward and separates from the punch, and the part fits on the punch. The blank holder ring is pushed up by the unloading screw to remove the part from the punch, and the drawing forming is completed. Four steel lifting rings are set on the side end faces of the upper and lower die plates for lifting the tooling.

[0009] The second step: drilling. The tooling used in the drilling process is a "drill sleeve mold tire", which includes: a tire body and a fixed drill sleeve.

[0010] The tooling "mold with drill sleeve" uses the part profile as the positioning reference, places the part into the mold body, uses a hand drill along the fixed drill sleeve to drill a 1-φ5.2mm hole on the part, and uses a universal punching die to expand the 1-φ5.2mm hole into a 1-φ10mm hole, which is used as the bottom hole for stamping the convex edge in the third process.

[0011] The third step: stamping convex edge. The tooling used in the stamping convex edge process is the "convex edge die", which includes: upper template A, punch A, die A, lower template A, guide column A, guide sleeve A, fixing screw A, cylindrical pin A, lifting ring A, die handle A.

[0012] The tooling "convex edge die" can realize the convex edge hole forming of aluminum alloy sheet. The upper mold plate A and the lower mold plate A are made of Q235-AF steel material; the punch A and the die A are made of 45# steel material, heat treated to a hardness of 35-39HRC. The gap between the punch and the die is 1.1 times the material thickness. The manufacturing tolerance of the tooling profile is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm.

[0013] The die handle A and the upper template A, the punch A and the die A and the lower template A are all connected and fixed through the fixing screw A hole. The two guide sleeves A installed on the upper template A and the two guide pillars A installed on the lower template A adopt the H5 / h5 clearance fit, and the two guide pillars A play a limiting role. Before punching the convex edge, the die handle A, the upper template A and the punch A are driven upward by the punch press, so that the punch A is away from the die A, and the part rough material is placed on the die A, so that the part surface is fitted and fixed with the die A, and lubricating oil is evenly applied near the φ10mm hole on the part rough material and the working surface of the convex edge die.

[0014] When the "convex edge die" is working, step on the clutch device, the punch press moves downward instantly, the die handle A drives the upper die plate A and the punch A to move downward together, and the die is closed instantly. The punch A and the die A move relative to each other, and the part is formed by stamping the convex edge. When the die is opened, the punch A moves upward and separates from the die A, the part is attached to the die A, the convex edge hole is formed, the part is taken out with tweezers, and the stamping of the convex edge is completed. Four steel lifting rings A are set on the side end faces of the upper die plate A and the lower die plate A for lifting the tooling.

[0015] The fourth process is to cut the shape with a laser cutting machine. The tooling used in the laser cutting process is a "laser cutting fixture", which includes: a base plate, a laser cutting fixture body, a marking block, a marking block fixing screw, a marking block fixing pin, and a double-sided pressure plate.

[0016] The tooling "laser cutting fixture" described above has a base plate that acts as a stable support. The three marking blocks serve as positioning references and are fixed to the base plate by the marking block fixing screws and marking block fixing pins. The parts are mounted on the laser cutting fixture body and fixed by double-sided pressure plates, studs and nuts. First, the parts are positioned on the laser cutting fixture body by surface positioning, the double-sided pressure plates are aligned with the flange holes of the parts and buckled on the parts, the studs are inserted into the double-sided pressure plates and the flange holes of the parts, the nuts are tightened, and the parts are clamped on the laser cutting fixture body. The laser cutting machine cuts the theoretical outline of the side wall of the part according to the cutting program, and the part processing is completed.

[0017] Beneficial effects of the present invention:

[0018] By adopting a new combined manufacturing method to form aluminum alloy three-way and half-tube parts with complex profiles and convex edge holes, the cracking, wrinkling, inadequate forming, and many surface hammer marks caused by manual forming are avoided. The labor intensity and dimensional tolerance problems caused by manual shearing are avoided, and the surface quality of the parts is improved, and the surface roughness is increased to no more than Ra3.2μm. The parts formed by this method have a tire adhesion of less than 0.5mm, and the shape limit deviation meets ±0.5mm. The production cycle of processing one aluminum alloy three-way and half-tube part with a complex profile is shortened from 6 to 8 hours to 2 hours, and the scrap rate is reduced from 70% to 10%. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is the part appearance drawing;

[0020] Figure 2 This is the cross-sectional view of the drawing die;

[0021] Figure 3 It is the top view of the drawing die;

[0022] Figure 4 (a) is a drawing die parts diagram;

[0023] Figure 4(b) is the AA view of the drawing die;

[0024] Figure 5 (a) is a schematic diagram of a mold with a drill sleeve;

[0025] Figure 5(b) is the AA view of the mold with drill sleeve;

[0026] Figure 6 (a) is a front view of the convex edge mold;

[0027] Figure 6(b) is the AA view of the convex edge mold;

[0028] Figure 6(c) is a schematic diagram of the convex edge mold;

[0029] Figure 7(a) is a schematic diagram of a laser cutting fixture;

[0030] Figure 7(b) is the AA view of the laser cutting fixture.

[0031] In the figure: 1 upper template; 2 die; 3 pressure ring; 4 punch; 5 lower template; 6 guide pin; 7 guide sleeve; 8 unloading screw; 9 lifting ring; 10 die handle fixing screw; 11 cylindrical pin; 12 fixing screw; 13 die handle; 14 carcass; 15 fixed drill sleeve; 16 upper template A; 17 punch A; 18 die A; 19 lower template A; 20 guide pin A; 21 guide sleeve A; 22 fixing screw A; 23 cylindrical pin A; 24 lifting ring A, 25 die handle A; 26 bottom plate; 27 laser cutting fixture carcass; 28 marking block; 29 marking block fixing screw; 30 marking block fixing pin; 31 carcass fixing screw; 32 double-sided pressure plate; 33 stud; 34 nut. DETAILED DESCRIPTION

[0032] The present invention is further described below in conjunction with specific embodiments.

[0033] Embodiment 1:

[0034] This combined manufacturing method combines the advantages of deep drawing, drilling, convex edge stamping and laser cutting to efficiently manufacture complex aluminum alloy three-way half-tube parts with convex edge holes.

[0035] First, deep drawing is performed. Install the drawing die on the stamping hydraulic press, and use a crane or forklift to place the drawing die on a workbench or pad in the mold-closing state. Adjust the position of the die to ensure that the die handle is aligned with the die handle hole of the slider. When the die handle is fixed, manually lock the die handle hole so that the upper die plate of the drawing die is clamped and fixed on the slider; when the pressure plate is fixed, manually tighten the pressure plate screw and use the pressure plate to fix the lower die plate on the workbench. The slider of the stamping hydraulic press slides upward to separate the upper and lower dies of the drawing die. Before deep drawing, a test pressure is required, and lubricant is evenly applied to the front and back sides of the part raw material along the shape. Place a piece of test pressure raw material on the drawing die pressure ring to ensure uniform peripheral margin. Set the hydraulic press pressure and the depth of the first deep drawing test pressure according to the theoretical value. The slider moves downward, the mold is closed, and after the pressure is maintained for more than 5 seconds, the slider moves upward and the mold is opened. The ejector composed of the unloading screw and the pressure ring pushes the formed part upward to remove the test pressure part from the punch. After the parts are taken out, observe the deep drawing of the parts to see if wrinkles or cracks appear. Adjust the deep drawing test conditions: According to the material flow of the test parts, manually cut and trim the raw materials that have not been deep drawn, and appropriately remove the parts where the material flow is not smooth; if wrinkles appear, increase the blanking force; if cracks appear, reduce the blanking force or apply lubricating oil on the die and blanking ring. Through multiple press tests, and gradually increase the drawing depth until the final forming state of the drawing die used is reached, record the depth and blanking force of each forming, and determine the size and shape of the deep drawing raw materials. After the press test is successful, the parts are deep drawn and formed according to the forming process determined during the deep drawing test: according to the size, shape and blanking force of the raw materials obtained by the test, the parts are deep drawn one by one to make the parts reach the final forming state. When the hydraulic press is deep drawn multiple times, an intermediate annealing process can be added to eliminate the influence of cold work hardening.

[0036] The second step is to drill a 1-φ5.2mm hole on the part according to the drill sleeve die, and position and install the part on the die body through the profile. Use a handheld air drill to make the drill enter the fixed drill sleeve of the drill jig to drill a 1-φ5.2mm hole. The fixed drill sleeve acts as a guide for the drill. Use a 1-φ5.2mm center hole for positioning, and use a universal punching die to expand the 1-φ5.2mm hole into a 1-φ10mm hole, which is used as the bottom hole for the third process of stamping the convex edge. Use a scraper or a drill bit larger than the processed hole or a homemade tool to file and deburr the processed hole.

[0037] The third step is to stamp the convex edge. Place a washer on the workbench of the stamping equipment, and place the convex edge die on the washer in the mold closing state to ensure that the die handle is aligned with the die handle hole of the slider. Slide the press slider down to make the die handle of the upper die of the convex edge die enter the die handle hole on the slider, manually lock the die handle hole to clamp the die handle, so that the upper mold plate is installed and fixed on the press slider, use the pressure plate to press the lower mold plate of the convex edge die, tighten the pressure plate screw to fix the lower mold plate on the press workbench, slide the press slider up, return the slider to the starting position, and separate the upper and lower molds. Start the motor of the press. Manually position the part on the die 18 through the molding surface, and after both hands leave the mold closing surface, step on the clutch device to realize one-time stamping convex edge forming. After taking out the part with tweezers, check the quality of the part's convex edge hole. If the quality of the part is qualified after the convex edge is stamped, the rough material of other parts will be stamped.

[0038] The fourth step is to use a crane to hoist the laser cutting fixture onto the cutting platform of the laser cutting machine, and use the machine tool pressure plate to fix the base plate 2 on the machine tool platform. The parts are positioned on the laser cutting fixture body 27 by the profile positioning, and are fixed by the double-sided pressure plate, studs and nuts to fix the rough parts to be processed tightly on the surface of the cutting fixture. Use the three marking blocks as the positioning reference to align the coordinate system so that the coordinate system of the machine tool coincides with the programming coordinate system. Adjust the laser head away from the mold and parts, test run the laser cutting program, and conduct the formal cutting process after confirming that there are no errors in the running trajectory and no collisions. Press the start switch on the machine tool operation panel to automatically perform the cutting operation and cut the theoretical outline of the part. The cutting operation is terminated, the nuts, studs and the clamping force of the double-sided pressure plate are unloaded, and the parts are removed from the laser cutting fixture. The limit deviation of the part's outer size meets ±0.5mm, and the parts are delivered qualified.

[0039] Embodiment 2:

[0040] A method for manufacturing a complex aluminum alloy tee half-tube component with a convex edge hole, the steps are as follows:

[0041] Step 1: Deep drawing. The tooling used in the deep drawing process is the "drawing die", which includes: upper template 1, concave die 2, blank holder 3, punch 4, lower template 5, guide pin 6, guide sleeve 7, unloading screw 8, lifting ring 9, die handle fixing screw 10, cylindrical pin 11, fixing screw 12, die handle 13.

[0042] The tooling "drawing die" can realize the deep drawing of aluminum alloy sheet. The upper template 1 and the lower template 5 are made of Q235-AF steel; the die 2, the blank holder 3 and the punch 4 are made of Cr12MoV steel, which is heat treated to a hardness of 59-62HRC. The gap between the die 2 and the punch 4 is 1.1 times the material thickness. The manufacturing tolerance of the "drawing die" tooling profile is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm. The punch 4 and the lower template 5 of the "drawing die" tooling are connected and fixed by hole matching, and the die 2 and the upper template 1 are connected and fixed by hole matching. The unloading screw 8 and the blank holder 3 form a pusher, which always pushes the formed parts up to play a role in unloading. The two guide sleeves 7 installed on the upper template 1 and the two guide pillars 6 installed on the lower template 5 adopt H5 / h5 clearance matching, and the two guide pillars 6 play a limiting role. Before drawing, the blank holder 3 is pushed up by the unloading screw 8, so that the blank holder 3 is away from the lower template 5 and placed above the punch 4, with the distance from the lower template 5 greater than the part surface height, and the part rough material is placed on the blank holder 3, and lubricating oil is evenly applied to the front and back sides of the part rough material along the theoretical shape.

[0043] When the "drawing die" is working, the stamping hydraulic press moves downward, and the die handle 13 drives the upper die plate 1 and the die 2 to move downward together, and the die begins to close. The die 2 continues to move downward until it fits with the blank holder 3 and drives the blank holder 3 to move downward together. The sheet metal contacts the punch 4, and the part begins to be formed. The upper die plate 1, the die 2, the blank holder 3, the punch 4, and the lower die plate 5 slide with the guide sleeve 7 and the guide column 6. The sheet metal is pushed up by the punch 4 and enters the groove of the die 2 until the blank holder 3 moves down to the lower die plate 5, and the closing of the die is completed. When the die is opened, the die 2 moves upward and separates from the punch 4, and the part fits on the punch 4. The blank holder 3 is pushed up by the unloading screw 8 to remove the part from the punch 4, and the drawing forming is completed. Four steel lifting rings 9 are respectively set on the side end faces of the upper die plate 1 and the lower die plate 5 for lifting the tooling.

[0044] The second step: drilling. The tooling used in the drilling process is a "drill sleeve mold tire", and the "drill sleeve mold tire" tooling includes: a tire body 14 and a fixed drill sleeve 15.

[0045] The tooling "mold with drill sleeve" uses the part profile as the positioning reference, places the part into the carcass 14, uses a hand drill along the fixed drill sleeve 15 to drill a 1-φ5.2mm hole on the part, and uses a universal punching die to expand the 1-φ5.2mm hole into a 1-φ10mm hole, which is used as the bottom hole for punching the convex edge in the third process.

[0046] The third step: stamping convex edge. The tooling used in the stamping convex edge process is the "convex edge die", which includes: upper die plate A16, punch die A17, die die A18, lower die plate A19, guide column A20, guide sleeve A21, fixing screw A22, cylindrical pin A23, lifting ring A24, die handle A25.

[0047] The tooling "convex edge die" can realize the forming of the convex edge hole of the aluminum alloy sheet. The upper die plate A16 and the lower die plate A19 are made of Q235-AF steel material; the punch A17 and the die A18 are made of 45# steel material, heat treated to a hardness of 35-39HRC. The gap between the punch and the die is 1.1 times the material thickness. The manufacturing tolerance of the tooling profile is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm.

[0048] The die handle A25 and the upper die plate A16, the punch A17 and the die A18 and the lower die plate A19 are all connected and fixed through the fixing screw A22 hole. The two guide sleeves A21 installed on the upper die plate A16 and the two guide pillars A20 installed on the lower die plate A19 adopt the H5 / h5 clearance fit, and the two guide pillars A20 play a limiting role. Before punching the convex edge, the die handle A25, the upper die plate A16 and the punch A17 are driven upward by the punch press, so that the punch A17 is away from the die A18, and the part rough material is placed on the die A18, so that the part surface is fitted and fixed with the die A18, and lubricating oil is evenly applied near the φ10mm hole on the part rough material and the working surface of the convex edge die.

[0049] When the "convex edge die" is working, step on the clutch device, the punch press moves downward instantly, the die handle A25 drives the upper die plate A16 and the punch A17 to move downward together, and the die is closed instantly. The punch A17 and the die A18 move relative to each other, and the part is formed by stamping the convex edge. When the die is opened, the punch A17 moves upward and separates from the die A18, the part is attached to the die A18, the convex edge hole is formed, the part is taken out with tweezers, and the stamping of the convex edge is completed. Four steel lifting rings A24 are set on the side end faces of the upper die plate A16 and the lower die plate A19 for lifting the tooling.

[0050] The fourth process is to cut the shape with a laser cutting machine. The tooling used in the laser cutting process is a "laser cutting fixture", which includes: a base plate 26, a laser cutting fixture body 27, a marking block 28, a marking block fixing screw 29, a marking block fixing pin 30, and a double-sided pressing plate 32.

[0051] The tooling "laser cutting fixture" described above has a base plate 26 that acts as a stable support, and three marking blocks 28 that serve as positioning references are fixed to the base plate 26 by means of marking block fixing screws 29 and marking block fixing pins 30. The parts are mounted on the laser cutting fixture body 27 and fixed by means of double-sided pressing plates 32, studs 33 and nuts 34. First, the parts are positioned on the laser cutting fixture body 27 by means of the profile, the double-sided pressing plates 32 are aligned with the flange holes of the parts and buckled onto the parts, the studs 33 are inserted into the double-sided pressing plates 32 and the flange holes of the parts, the nuts 34 are tightened, and the parts are clamped on the laser cutting fixture body 27. The laser cutting machine cuts the theoretical outline of the side wall of the part according to the cutting program, and the part processing is completed.

Claims

1. A method for manufacturing a complex aluminum alloy tee half-tube component with a convex edge hole, characterized in that: Here are the steps: Step 1: deep drawing; the tooling used in the deep drawing process is a "drawing die", which includes: an upper die plate (1), a concave die (2), a blank holder (3), a punch (4), a lower die plate (5), a guide post (6), a guide sleeve (7), a discharge screw (8), a lifting ring (9), a die handle fixing screw (10), a cylindrical pin (11), a fixing screw (12), and a die handle (13); The punch (4) and the lower die plate (5) of the "drawing die" tooling are connected and fixed by hole matching, the die (2) and the upper die plate (1) are connected and fixed by hole matching, and the unloading screw (8) and the pressure ring (3) form a pusher, which always pushes the formed parts up to play the role of unloading; the two guide sleeves (7) installed on the upper die plate (1) and the two guide pillars (6) installed on the lower die plate (5) adopt H5 / h5 clearance matching, and the two guide pillars (6) play a limiting role; When the "drawing die" is working, the stamping hydraulic press moves downward, the die handle (13) drives the upper die plate (1) and the female die (2) to move downward together, and the die begins to close; the female die (2) continues to move downward until it fits with the blank holder (3) and then drives the blank holder (3) to move downward together, the sheet metal contacts the punch (4), and the part begins to be formed. The upper die plate (1), the female die (2), the blank holder (3), the punch (4), and the lower die plate (5) slide in a limited manner through the guide sleeve (7) and the guide column (6), and the sheet metal is pushed up by the punch (4) into the groove of the female die (2) until the blank holder (3) moves down to the lower die plate (5), and the closing of the die is completed; when the die is opened, the female die (2) moves upward and separates from the punch (4), and the part fits on the punch (4). The blank holder (3) is pushed up by the unloading screw (8), and the part is removed from the punch (4), and the drawing forming is completed; The second step: drilling; the tooling used in the drilling process is a "drill set mold tire", and the "drill set mold tire" tooling includes: a tire body (14), a fixed drill sleeve (15); The tooling "die with drill sleeve" uses the part profile as a positioning reference, places the part into the die body (14), uses a hand drill along a fixed drill sleeve (15) to drill a 1-φ5.2mm hole on the part, and uses a universal punching die to expand the 1-φ5.2mm hole into a 1-φ10mm hole, which is used as the bottom hole for punching the convex edge in the third process; Step 3: stamping the convex edge; the tooling used in the stamping convex edge process is a "convex edge die", which includes: an upper die plate A (16), a punch die A (17), a die die A (18), a lower die plate A (19), a guide post A (20), a guide sleeve A (21), a fixing screw A (22), a cylindrical pin A (23), a lifting ring A (24), and a die handle A (25); The die handle A (25) and the upper die plate A (16), the punch A (17) and the die A (18) and the lower die plate A (19) are all connected and fixed by means of the holes of the fixing screws A (22); the two guide sleeves A (21) installed on the upper die plate A (16) and the two guide pillars A (20) installed on the lower die plate A (19) are matched with a clearance of H5 / h5, and the two guide pillars A (20) play a role of limiting; When the "convex edge die" is working, the clutch device is stepped on, the punch press moves downward instantly, the die handle A (25) drives the upper die plate A (16) and the punch A (17) to move downward together, and the die is instantly closed; the punch A (17) and the die A (18) move relative to each other, and the part is formed by stamping and convex edge; when the die is opened, the punch A (17) moves upward and separates from the die A (18), the part is attached to the die A (18), the convex edge hole is formed, the part is taken out by tweezers, and the stamping and convex edge is completed; The fourth process is to cut the shape using a laser cutting machine; the tooling used in the process of cutting the shape using a laser cutting machine is a "laser cutting fixture", and the "laser cutting fixture" tooling includes: a base plate (26), a laser cutting fixture body (27), a marking block (28), a marking block fixing screw (29), a marking block fixing pin (30), and a double-sided pressing plate (32); The tooling "laser cutting fixture" has a base plate (26) that plays a role of stable support, and three marking blocks (28) that serve as positioning references and are fixed to the base plate (26) by means of marking block fixing screws (29) and marking block fixing pins (30); the parts are mounted on the laser cutting fixture body (27) and fixed by means of double-sided pressing plates (32), studs (33) and nuts (34); first, the parts are positioned on the laser cutting fixture body (27) by means of profile positioning, the double-sided pressing plates (32) are aligned with the flange holes of the parts and buckled onto the parts, the studs (33) are inserted into the double-sided pressing plates (32) and the flange holes of the parts, the nuts (34) are tightened, and the parts are clamped on the laser cutting fixture body (27); the laser cutting machine cuts the theoretical outer contour of the side wall of the parts according to the cutting program, and the parts are processed.

2. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with a convex edge hole as claimed in claim 1, characterized in that: The upper template (1) and the lower template (5) are made of Q235-AF steel material; The die (2), blank holder (3) and punch (4) are made of Cr12MoV steel material and are heat treated to a hardness of 59-62HRC; The gap between the concave die (2) and the convex die (4) is 1.1 times the material thickness; the manufacturing tolerance of the "drawing die" tooling surface is less than 0.1 mm, and the surface roughness is not greater than Ra6.3 μm.

3. A method for manufacturing a complex-profile aluminum alloy tee half-tube component with a convex edge hole as claimed in claim 1 or 2, characterized in that: In the first step, before deep drawing, the blank holder (3) is pushed up by the unloading screw (8), so that the blank holder (3) is away from the lower template (5) and placed above the punch (4), with the distance from the lower template (5) greater than the part surface height, and the part rough material is placed on the blank holder (3), and lubricating oil is applied to the front and back sides of the part rough material.

4. A method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 1 or 2, characterized in that: The upper mold plate A (16) and the lower mold plate A (19) are made of Q235-AF steel; the male mold A (17) and the female mold A (18) are made of 45# steel, heat-treated to a hardness of 35-39HRC; The clearance between the concave and convex dies is 1.1 times the material thickness; the manufacturing tolerance of the "convex edge die" tooling surface is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm.

5. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 3, characterized in that: The upper mold plate A (16) and the lower mold plate A (19) are made of Q235-AF steel; the male mold A (17) and the female mold A (18) are made of 45# steel, heat-treated to a hardness of 35-39HRC; The clearance between the concave and convex dies is 1.1 times the material thickness; the manufacturing tolerance of the "convex edge die" tooling surface is less than 0.1mm, and the surface roughness is not greater than Ra6.3μm.

6. A method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 1, 2 or 5, characterized in that: In the third step, before punching the convex edge, the die handle A (25), the upper die plate A (16) and the punch A (17) are driven upward by the punch press, so that the punch A (17) is away from the die A (18), the part blank is placed on the die A (18), the part surface is fitted and fixed with the die A (18), and lubricating oil is applied near the φ10 mm hole on the part blank and the working surface of the convex edge die.

7. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 3, characterized in that: In the third step, before punching the convex edge, the die handle A (25), the upper die plate A (16) and the punch A (17) are driven upward by the punch press, so that the punch A (17) is away from the die A (18), the part blank is placed on the die A (18), the part surface is fitted and fixed with the die A (18), and lubricating oil is applied near the φ10 mm hole on the part blank and the working surface of the convex edge die.

8. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 4, characterized in that: In the third step, before punching the convex edge, the die handle A (25), the upper die plate A (16) and the punch A (17) are driven upward by the punch press, so that the punch A (17) is away from the die A (18), the part blank is placed on the die A (18), the part surface is fitted and fixed with the die A (18), and lubricating oil is applied near the φ10 mm hole on the part blank and the working surface of the convex edge die.

9. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 1, characterized in that: The upper template (1) and the lower template (5) are respectively provided with four steel lifting rings (9) on their side end faces, and the upper template A (16) and the lower template A (19) are respectively provided with four steel lifting rings A (24) on their side end faces for lifting tooling.

10. The method for manufacturing a complex-profile aluminum alloy tee half-tube component with convex edge holes as claimed in claim 3, characterized in that: The upper template (1) and the lower template (5) are respectively provided with four steel lifting rings (9) on their side end faces, and the upper template A (16) and the lower template A (19) are respectively provided with four steel lifting rings A (24) on their side end faces for lifting tooling.

Citation Information

Patent Citations

  • Forming method of tee joint half-tube part and compound punching die

    CN103752668A

  • Aluminum alloy annular sheet metal part combination manufacturing die and method

    CN114986178A

  • Method for controlling room-temperature forming springback defect of TC1 large-curvature titanium alloy half tube

    CN118477916A

  • Building integrated air type photohvoltaic-thermal collector

    KR1020220055623A