Multi-pass progressive bending forming method for high-rib wallboard filled with special materials and high-rib wallboard
Through the multi-pass progressive bending forming method of filling high-rubic wall panels with special materials, the problems of low dimensional accuracy and concentrated stress during the bending forming process of aluminum alloy wall panels are solved, and high-quality wall panel molding is achieved to meet aerospace fuel tank requirements for the appliance.
Patent Information
- Application Number
- CN202411254879.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-09
- Publication Date
- 2024-11-22
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
The prior art has cracks and necking problems caused by low dimensional accuracy, high processing difficulty, and concentrated stress during the bending and forming process of aluminum alloy wall panels, which leads to unstable product quality and is difficult to meet the requirements of fuel storage tanks for aerospace vehicles. .
Multi-pass progressive bending molding method using special materials to fill high-strength wall panels, the bending molding process parameters are calculated through grid processing, finite element simulation and variational method-minimum potential energy principle, and follow-up adjustable bending The machine performs multi-pass bending molding to control the gap between the filler and the ribs and bending force to avoid deformation caused by mechanical stress release.
It improves product quality stability, reduces processing difficulty, and meets the requirements of the curvature and straightness of the wall panels, with a pass rate of 99%. The surface of the wall panels is smooth and defect-free, meeting the needs of aerospace vehicles.
Smart Images

Figure CN118989878A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of aerospace metal processing and manufacturing technology, and relates to a bending forming method of a high-rib wall panel, and in particular to a multi-pass progressive bending forming method of a high-rib wall panel filled with special materials and a high-rib wall panel. Background Art
[0002] In recent years, with the rapid development of my country's aerospace technology, the fuel tanks and oxidizer tanks of aerospace vehicles are mostly made of aluminum alloy plates. The tank is made of multiple wall panels welded together to form a tank cylinder. Nowadays, in order to consider the lightweight of rockets and increase the payload, thin-skin aluminum alloy wall panels with reinforcement ribs can greatly reduce the mass while ensuring the overall structural strength.
[0003] The specific product of thin-skin aluminum alloy wall panel with reinforcing ribs is a wall panel with a maximum thickness of 19mm, and the rib height of 16mm is obliquely orthogonal to the thickness of the skin area of 3mm, the rib width is relatively narrow, about 9-12mm, and the root radius at the intersection of thin and thick parts is small, R3-5. The product requires a forming curvature of R1648mm. The high-rib thin-skin variable grid structure CNC milling wall panel is difficult to form. During the forming process, it is very easy to cause stress concentration due to the instability of the high-rib thin skin and the small root radius, resulting in buckling and necking of the ring ribs, resulting in product cracking or insufficient forming, resulting in product failure to meet the standards.
[0004] In terms of existing technology, roll forming, press bending, shot peening, creep forming and plate bending milling are usually used at home and abroad. Plate bending milling refers to bending a flat sheet and then milling it to manufacture a thin-skinned wall panel with ribs. It faces the problems of low dimensional accuracy caused by thin-wall flutter during milling, difficulty in milling on curved surfaces, breaking the original internal stress balance of the wall panel after processing, and serious deformation of parts. While choosing to mill a thin-skinned wall panel with ribs from a flat sheet and then roll forming it can greatly reduce the difficulty of milling, it is difficult to control the changes in material thickness caused by elastic-plastic deformation during rolling, deformation of the rib grid or wrinkling and puncturing of the thin wall. In the subsequent shaping process, cracks, uneven surfaces, and damage such as upsetting and necking at the thin rib stress points often occur. The product quality stability is poor, and the surface accuracy of the grid wall panel parts such as curvature, roundness and straightness is poor, which directly affects the welding difficulty of the tank body. The bending process is one of the difficult problems of liquid-fuel rockets manufactured after assembly welding. The core of the bending forming process is how to reduce the dimensional and structural damage to the wall panels during processing and control the errors and mechanical stress concentration caused by the springback of the wall panels after processing. Summary of the invention
[0005] The invention provides a multi-pass progressive bending forming method of a high-rib wall panel filled with a special material and a high-rib wall panel, so as to overcome the defects of the prior art.
[0006] To achieve the above object, the present invention adopts the following technical solutions:
[0007] A multi-pass progressive bending method for a high-rib wall panel filled with a special material, characterized in that it includes the following steps: S1, gridding an aluminum alloy flat blank to obtain a wall panel with ribs; S2, placing fillers into the wall panel and covering the aluminum alloy plate; S3, performing multi-pass bending to form the wall panel with the fillers; wherein the filler material is determined according to Young's modulus, the filler height is determined by finite element simulation, the bending forming process parameters are calculated using the variational method-minimum potential energy principle, and the gap between the filler and the ribs is calculated using the neutral layer offset principle during the bending process.
[0008] To optimize the above technical solutions, the specific measures taken also include:
[0009] Furthermore, the method for determining the filler material is: calculating the ideal Young's modulus of the filler, and then selecting the filler material according to the ideal Young's modulus;
[0010] The calculation formula for the ideal Young's modulus of the filler is:
[0011]
[0012] In the formula, is the ideal Young's modulus of the filler, E1 is the Young's modulus of the panel, I1 is the moment of inertia of the rib-skin unit in the panel, and I2 is the moment of inertia of the filler.
[0013] Furthermore, the method for determining the filler height is: simulating the bending process of the wall panel with different filler heights through finite element simulation, when the stress peak in the finite element simulation result no longer changes with the filler height, the filler height at this time is the filler height to be determined.
[0014] Furthermore, the bending forming is carried out by a follow-up adjustable bending machine; the follow-up adjustable bending machine includes an upper die group and a follow-up lower die group; the top of the upper die group is connected to a press, and the follow-up lower die group is located below the upper die group; the follow-up lower die group includes two lower die frames with adjustable spacing and a follow-up lower die installed on the lower die frame and capable of rotating relative to the lower die frame; the wall panel is placed between the upper die group and the two follow-up lower dies; the wall panel is bent under the downward pressure applied by the upper die group, and the follow-up lower die rotates accordingly.
[0015] Furthermore, the bending forming process parameters include bending force, which is calculated as follows:
[0016] Π=W P -U 弹 -U 塑 ;
[0017] Where Π is the total potential energy of the system; WP U is the work done by the bending force in the height direction of the sheet; 弹 is the elastic internal potential energy of the panel during the bending process; U 塑 is the internal potential energy of the panel during plastic deformation;
[0018] The system uses a Cartesian coordinate system, where the x direction is the direction extending the rib length and parallel to the skin, the y direction is perpendicular to the rib elevation and parallel to the skin, and the z direction is perpendicular to the skin and parallel to the rib height. The origin of the coordinate system is set at the centroid of the bottom skin.
[0019]
[0020] Where D1 and D2 are the bending stiffness of the wall panel and filler, respectively. E1 and E2 are the Young's modulus of the wall plate and filler, respectively; t1 and t2 are the heights of the ribs and filler, respectively; ν1 and ν2 are the Poisson's ratios of the wall plate and filler, respectively; ω1 and ω2 are the deflection functions of the wall plate and filler, respectively, which are used to represent the displacement of the top of the rib after instability;
[0021] The rib part of the panel is simplified to three-side fixed supports, and the deflection function of the panel is expressed as:
[0022]
[0023] The boundary conditions of the deflection function of the wall plate are:
[0024]
[0025] The packing part is simplified to three-side simply supported constraints, and the deflection function of the packing is expressed as:
[0026]
[0027] The boundary condition of the packing deflection function is:
[0028]
[0029] The grid of the wall panel is an oblique orthogonal grid, a is the length of the grid; b is the height of the wall panel;
[0030]
[0031] Where, P is the bending force;
[0032] Let δΠ=0, take the minimum value Π min , the bending force is calculated.
[0033] Furthermore, the bending forming process parameters also include a lower die spacing between two follower lower dies, which is calculated as follows:
[0034]
[0035] In the formula, σ b is the tensile strength of the siding material; α is the arc of the lower die center; R is the bending radius of the siding;
[0036] The curvature of the lower die center is calculated based on the bending force, and the lower die spacing is calculated based on the curvature of the lower die center.
[0037] Furthermore, the calculation method of the gap between the filler and the rib is: using the axial mechanical balance model, a balance equation is established for the upper and lower sides of the neutral plane during the bending process of the wall panel:
[0038] F b =F t =F 弹 +F 塑 ;
[0039] In the formula, F b F is the tension in the lower part of the neutral layer; t is the pressure above the neutral layer; F 弹 is the compressive stress in the elastic deformation zone; F 塑 is the compressive stress in the plastic deformation zone;
[0040]
[0041] Where b1 is the height of the neutral layer; b s is the cut-off height of elastic deformation on one side of the neutral layer, ρ is the target curvature radius of the wall panel; σ s is the yield strength of the wallboard material; E1 and E2 are the Young's modulus of the wallboard and filler respectively; P is the compressive bending force; the grid of the wallboard is an oblique orthogonal grid, a is the length of the grid; b is the height of the wallboard; c is the thickness of the rib; t1 is the height of the rib; s0 is the gap between the filler and the rib; s1 is the height difference between the filler and the rib;
[0042]
[0043] Where N is the plastic strengthening modulus of the siding material;
[0044]
[0045] The gap between the filler and the ribs is calculated using the equilibrium equation.
[0046] Furthermore, the method for the multi-pass bending forming is: taking the center of the inner surface of the wall panel as a reference, drawing bending lines at equal intervals on both sides along the circumferential direction, and performing multi-pass progressive bending forming according to the bending lines.
[0047] Furthermore, the smooth surface of the gridded wall panel is covered with a film, and then fillers are placed; after bending and forming, the wall panel is compared with the theoretical sample size of the inner surface and then pressurized point by point for correction.
[0048] The invention also provides a high-rib wall panel made by the above method.
[0049] The beneficial effects of the present invention are as follows: the present invention provides a multi-pass progressive bending forming method and a high-ribbed wall panel filled with special materials, which not only optimizes the bending processing operation method of thin-skinned aluminum alloy wall panels with reinforcing ribs, but also avoids deformation caused by the release of mechanical stress inside the panel after curved surface milling, or cracks, surface punctures and wrinkles during the bending process after flat milling. Under the condition that the curvature of the aluminum alloy wall panel meets the requirements, there is no puncture or wrinkling inside, and the reinforcing ribs have no upsetting and necking, which improves the stability of product quality, can ensure stable and reliable batch production in the product manufacturing process, and can meet the use requirements of fuel tanks and oxidizer tanks of aerospace vehicles. The present invention also provides a calculation method for filler-related parameters, bending forming process parameters, etc., which can greatly reduce the processing difficulty of wall panel bending forming, and reduce the correction amount by 80%; at the same time, it also improves the success rate of bending forming, and the qualified rate reaches more than 99%. Through testing, the deviation between the actual curvature of the wall panel and the theoretical value is ≤0.8mm, the generatrix straightness is ≤1.5mm, and the surface of the wall panel is smooth without scratches, unevenness, cracks and other surface defects. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 It is a flow chart of the multi-pass progressive bending forming method of high-rib siding filled with special materials;
[0051] Figure 2 It is a wall panel with reinforcing ribs after milling;
[0052] Figure 3 It is a schematic diagram of a cross-section of a wall panel;
[0053] Figure 4 It is a structural schematic diagram of a follow-up adjustable bending machine;
[0054] Figure 5 It is a schematic diagram of the bending of the wall panel;
[0055] Figure 6 It is a schematic diagram of the structure of ribs and fillers;
[0056] Figure 7 It is a schematic diagram of the three-dimensional structure of ribs and fillers;
[0057] Figure 8 Simplified boundary diagrams of ribs (left) and fillers (right). DETAILED DESCRIPTION
[0058] The specific implementation of the present invention is described below with reference to the accompanying drawings.
[0059] like Figure 1 As shown, the present invention provides a multi-pass progressive bending forming method for a high-rib wall panel filled with a special material, comprising the following steps:
[0060] Step 1: hoist the aluminum alloy flat blank onto the milling equipment for mesh processing to obtain a ribbed wall panel, such as Figure 2 and 3 shown.
[0061] Among them, the length of the aluminum alloy flat blank is 800-5000mm, the width is 800-5000mm, the height is 1-50mm, and the material is 2A12, 2A14, 2219 and other aluminum alloy plates. The hoisting adopts the local vacuum adsorption method to clamp, and the hydraulic gantry crane system is used to load and unload materials and complete the grid milling of the blank. After milling, the length / width of the ribs of the wall panel is 10-100mm, the height is consistent with the overall wall panel, and the height of the bottom skin of the grid area is 2-5mm. The grid shape is an isosceles right triangle and a rectangle. The waist of the right triangle is 100-500mm, and the side length of the rectangle is 100-500mm. Each external chamfer is a C chamfer with a size of 0.5-2mm, and each internal chamfer is an R chamfer with a size of 2-20mm.
[0062] In this specific embodiment, an aluminum alloy flat plate with a length of 800mm, a width of 800mm, a thickness of 21mm, and a texture of 2219-T8 is selected as the blank. This material is a high-strength hard aluminum that has good plasticity under high temperature and high pressure. The selected aluminum alloy flat plate blank is clamped by a local vacuum adsorption method and hoisted on the milling equipment using a hydraulic gantry crane system. In the milling process, the two planes are first milled, and the surface roughness is ≤3.6. Figure 2 and 3 As shown, evenly distributed rectangular grids 12 and isosceles right triangle grids 13 are milled, the ribs 14 constituting the grids are 10 mm wide, and the height is 20 mm, which is consistent with the overall height of the wall panel 11. The thickness of the grid bottom skin 17 is 3 mm, the fillet 16 is 10 mm, the chamfer is 2 mm, and the thickness of the welding area 15 around the wall panel is 6 mm.
[0063] Step 2: Cover the smooth surface of the gridded wall panel with a film to prevent scratches and damage to the workpiece surface during subsequent processing. The film material includes but is not limited to polyethylene.
[0064] Step 3: Put filler into the wall panel and cover it with aluminum alloy plate.
[0065] The filler is polyvinyl chloride, polyurethane, etc. The shape of the filler is the same as the mesh shape produced by milling, and the gap between the filler and the rib is ≤0.5mm, and the gap between the filler and the skin fillet is ≤0.5mm. Covering the pressure area with a thin aluminum alloy plate can prevent scratches or damage to the wall panel and the mold during the subsequent bending process. Specifically, the thin aluminum alloy plate covers the entire bending area and its size is consistent with the size of the upper and lower mold surfaces of the bending machine.
[0066] Step 4: hoist the wall panel with filler onto the bending equipment for multiple bending steps.
[0067] Bending is done with a follow-up adjustable bending machine. Figure 4 As shown, the follow-up adjustable bending machine includes an upper die set and a follow-up lower die set. The top of the upper die set is connected to the press, and the follow-up lower die set is located below the upper die set. There is a working area between the upper die set and the follow-up lower die set for placing the wall panel. The upper die set includes an upper die frame 211, an upper die connecting plate 212, an upper die 213 and an upper die fastening bolt 214. The top of the upper die frame 211 is connected to the press through the upper die connecting plate 212, and the bottom is connected to the upper die 213 and fixed by the upper die fastening bolt 214. The upper die 213 comes into contact with the wall panel in the working area. The upper die 213 is equipped with multiple sizes such as R20, R100, and R700. Its surface has different treatment methods such as smooth, anti-slip pattern, and polyethylene film, which is suitable for parts of different sizes, materials, and structures. The lower die set includes a lower die base 221, a guide rail 222, a lower die frame 223, a lower die fastening bolt 224 and a follow-up lower die 225. The lower die base 221 is connected to the force-bearing surface of the press. The guide rail 222 is placed in the T-shaped slide groove of the lower die base 221. The lower die frame 223 contacts the guide rail 222 and is placed in the T-shaped groove of the lower die base 221 and is fixed by the lower die fastening bolts 224. The follower lower die 225 is placed in the cylindrical groove at the upper end of the lower die frame 223 and hinged. During the processing, it is ensured that it can be stably installed on the lower die frame 223 and the contact surface can be rotated with the deformation of the wall panel to reduce the impact and scratches during the molding process, thereby ensuring the molding quality. In order to facilitate the adjustment of the lower die frame 223, a ruler 226 with a 0 line is fixed on the side of the lower die base 221, and the 0 line is aligned with the geometric center of the upper die frame 211. Figure 5 As shown, when bending, the wall panel is placed between the upper die set and two follower lower dies 225. The wall panel is bent under the downward pressure applied by the upper die set, and the follower lower dies 225 rotate therewith.
[0068] The specific method of multi-pass bending forming is: according to the measured length of the wall panel, calculate the center of the inner surface of the wall panel. Take the center of the inner surface of the wall panel as the reference, and draw bending lines at equal intervals on both sides along the circumferential direction. Specifically, mark the serial numbers on the upper and lower ends of the heading, and the position of the marked serial numbers is parallel to the heading and perpendicular to the circumferential direction. Connect the corresponding upper and lower marked serial numbers to get the bending line. The bending line spacing is 100mm. Adjust the lower die spacing according to the size and thickness of the wall panel and ensure that its geometric center is aligned with the 0 line of the ruler. Place the wall panel between the upper die set and the two follow-up lower dies, and perform multi-pass progressive bending forming according to the bending line. During the process, control the forming curvature and gate pressure marks, and the amount of pressure each time is 2mm.
[0069] The hoisting adopts the local vacuum adsorption method to clamp, and the hydraulic gantry crane system is used to load and unload materials and complete the bending process of the wall panels. The wall panels are bent in multiple passes in a 3000-5000T hydraulic bending machine. The center angle after bending is 30-120° and the arc radius is 500-2000mm.
[0070] Step 5: Compare the wall panel with the theoretical sample size of the inner surface and perform point-by-point pressure correction.
[0071] Specifically, the bent wall panel is pressurized point by point from both ends, with each press of 1 to 1.5 mm. A thin aluminum alloy plate is used to cushion the pressure area so that the pressure at each point can be evenly distributed. At the same time, it is compared with the inner surface theoretical scale in real time to ensure that the wall panel is bent and fitted with the inner surface theoretical scale at both ends, the gap between the middle part and the inner surface theoretical scale is 0 to 5 mm, and the generatrix straightness is ≤ 1.5 mm, so that the curvature of the wall panel meets the requirements, there is no puncture or wrinkling inside, and the reinforcement ribs are not deformed.
[0072] In the above method, the filler material is determined according to Young's modulus, the filler height is determined by finite element simulation, the bending forming process parameters are calculated using the variational method-minimum potential energy principle, and the gap between the filler and the rib is calculated using the neutral layer offset principle during the bending process.
[0073] Specifically, The method for determining the filler material is :During the bending process, the deformation of the filler directly affects the transmission of pressure, and ultimately affects the quality of the forming results. The Young's modulus of the filler determines the ease of its deformation. If the filler is too hard, it will cause the skin to wrinkle or damage the fillet. If the filler is too soft, the pressure cannot be effectively transmitted, resulting in insufficient skin forming and lack of support for the ribs. In the bending process, in order to ensure that the bottom skin is fully formed, it is necessary to ensure that the upper mold contacts the upper surface of the filler first during the downward pressure process, so that the bending force is preferentially transmitted to the bottom skin. In order to ensure the coordinated deformation between the ribs and the wall panels, the ideal Young's modulus of the filler is first calculated, and then the filler material is selected according to the ideal Young's modulus.
[0074] The calculation formula for the ideal Young's modulus of the filler is:
[0075]
[0076] In the formula, is the ideal Young's modulus of the filler, E1 is the Young's modulus of the panel, I1 is the moment of inertia of the rib-skin unit in the panel (i.e. the inverted T-shaped structure composed of the ribs and the skin in the panel), and I2 is the moment of inertia of the filler.
[0077] The packing height is determined by :The finite element simulation is used to simulate the bending process of the wall panels with different filler heights. When the filler height increases to slightly higher than the ribs, the neutral layer at the skin no longer changes, the deformation no longer increases, and the deformation deflection of the filler reaches the extreme value under the process parameters. When the stress peak value (i.e., the CFNM interface pressure peak value) in the finite element simulation results no longer changes with the filler height, the filler height to be determined at this time.
[0078] The bending forming process parameters include the bending force, which is calculated as follows: : The total potential energy of the system is derived from the work done by all forces during the bending process:
[0079] Π=W P -U 弹 -U 塑
[0080] Where Π is the total potential energy of the system; W P U is the work done by the bending force in the height direction of the sheet; 弹 is the elastic internal potential energy of the panel during the bending process (i.e., the elastic potential energy of the elastic deformation of the rib-filler during the deformation process); U 塑 It is the internal potential energy of the wall panel during the plastic deformation process (i.e. the plastic potential energy generated by the plastic stress during the deformation of the ribs).
[0081] When the system reaches the equilibrium limit, its total potential energy is the smallest, that is, when δΠ=0 is satisfied, the critical load in the bending process, that is, the bending force of the bending process, can be determined.
[0082] like Figures 6 to 8 As shown, the system adopts a Cartesian coordinate system, the x direction is the direction extending the rib length and parallel to the skin, the y direction is the direction perpendicular to the rib facade and parallel to the skin, the z direction is perpendicular to the skin and parallel to the rib height, and the origin of the coordinate system is set at the centroid of the bottom skin.
[0083]
[0084] Where D1 and D2 are the bending stiffness of the wall panel and filler, respectively. E1 and E2 are the Young's modulus of the wall plate and filler, respectively; t1 and t2 are the heights of the ribs and filler, respectively; ν1 and ν2 are the Poisson's ratios of the wall plate and filler, respectively; ω1 and ω2 are the deflection functions of the wall plate and filler, respectively, which are used to represent the displacement of the top of the rib after instability;
[0085] like Figure 8 As shown in the figure, the rib part of the wall panel is simplified to three-side fixed supports, and the deflection function of the wall panel is expressed as:
[0086]
[0087] The boundary conditions of the deflection function of the wall plate are:
[0088]
[0089] The packing part is simplified to three-side simply supported constraints, and the deflection function of the packing is expressed as:
[0090]
[0091] The boundary condition of the packing deflection function is:
[0092]
[0093] The grid of the wall panel is an oblique orthogonal grid, a is the length (width) of the grid, and is the height of the wall panel.
[0094]
[0095] Where P is the bending force (i.e. the upper die bending force).
[0096] Let δΠ=0, take the minimum value Π min At this time, the internal force does not do work on the lateral deflection of the reinforcement, that is, the wall panel will not produce tension or lateral bending to cause reinforcement instability, and the compressive bending force is calculated.
[0097] The bending forming process parameters also include the die spacing between the two follower dies, which can be calculated as follows: : During the bending process, the downward pressure load is partially differentiated in the direction of the positive pressure to simplify it into the downward pressure acting on the center of the rib-filler unit:
[0098]
[0099] In the formula, σ b is the tensile strength of the siding material; α is the arc of the lower die center; R is the bending radius of the siding.
[0100] The arc of the lower die center is calculated based on the bending force. The arc of the lower die center refers to the angle between the bending center of the wall panel and the two follow-up lower dies, such as Figure 5 Then the lower die spacing is calculated based on the lower die center arc.
[0101] The calculation method of the gap between filler and rib is: :Using the axial mechanical equilibrium model, the equilibrium equations are established for the upper and lower sides of the neutral plane during the bending process of the wall panel. Specifically, when the deformation increases, the compressive bending force on the top of the rib increases, and a part of the top of the rib undergoes plastic deformation. The pressure on the upper part of the neutral layer is divided into two parts: the compressive stress in the elastic deformation zone and the compressive stress in the plastic deformation zone. The pressure on the upper part of the neutral layer and the tensile force on the lower part of the neutral layer are balanced when the resultant force is zero, so the equilibrium equation is:
[0102] F b =F t =F 弹 +F 塑
[0103] In the formula, F b F is the tension in the lower part of the neutral layer; t is the pressure above the neutral layer; F 弹 is the compressive stress in the elastic deformation zone; F 塑 is the compressive stress in the plastic deformation zone.
[0104] Starting from the neutral layer, the resultant force of the elastic stresses on the skin, ribs and filler is the compressive stress in the elastic deformation zone:
[0105]
[0106] Where b1 is the height of the neutral layer; b s is the cut-off height of elastic deformation on one side of the neutral layer, ρ is the target curvature radius of the wall panel; σ s is the yield strength of the wall panel material; E1 and E2 are the Young's modulus of the wall panel and filler respectively; P is the compressive bending force; the grid of the wall panel is an oblique orthogonal grid, a is the length (width) of the grid; b is the height of the wall panel; c is the thickness of the rib; t1 is the height of the rib; s0 is the gap between the filler and the rib, a-2s0 is the length (width) of the filler; s1 is the height difference between the filler and the rib, t1+s1 is the height t2 of the filler.
[0107] Starting from the neutral layer, the compressive stress in the plastic deformation zone is:
[0108]
[0109] Where N is the plastic strengthening modulus of the siding material.
[0110]
[0111] The gap between the filler and the ribs is calculated using the equilibrium equation.
[0112] When the panel undergoes stable elastic-plastic deformation, the filler transfers the load of the upper mold and limits the bending of the grid, balancing the deformation of the transverse ribs and the center of the skin, thereby improving the uniformity of the overall panel deformation. In this specific embodiment, the filler is polyurethane rubber, the filler height is 18 mm, the bending force is 373.87 MPa, the lower mold spacing is 160 mm, and the gap between the filler and the rib is 0.5 mm.
[0113] In the present invention, unless otherwise specified, the scientific and technical terms used herein have the meanings commonly understood by those skilled in the art. In addition, the reagents, materials and operating procedures used herein are reagents, materials and conventional procedures widely used in the corresponding fields.
[0114] It should be noted that the terms such as "upper", "lower", "left", "right", "front", "back", etc. cited in the invention are only for the convenience of description and are not used to limit the scope of implementation of the present invention. Changes or adjustments to their relative relationships should be regarded as the scope of implementation of the present invention without substantially changing the technical content.
[0115] Finally, it should be noted that the above are only preferred embodiments of the present invention and are not intended to limit the present invention. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art can still modify the technical solutions described in the aforementioned embodiments or replace some of the technical features therein by equivalents. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A multi-pass progressive bending forming method for high-rib wall panels filled with special materials, characterized in that: The following steps are involved: S1, meshing the aluminum alloy flat blank to obtain a siding with ribs; S2, putting filler into the wall panel and covering it with aluminum alloy plate; S3, performing multiple bending steps on the wall panel with fillers; Among them, the filler material is determined according to Young's modulus, the filler height is determined by finite element simulation, the bending forming process parameters are calculated using the variational method-minimum potential energy principle, and the gap between the filler and the rib is calculated using the neutral layer offset principle during the bending process.
2. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1 is characterized in that: The method for determining the filler material is: calculating the ideal Young's modulus of the filler, and then selecting the filler material according to the ideal Young's modulus; The calculation formula for the ideal Young's modulus of the filler is: In the formula, is the ideal Young's modulus of the filler, E1 is the Young's modulus of the panel, I1 is the moment of inertia of the rib-skin unit in the panel, and I2 is the moment of inertia of the filler.
3. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1 is characterized in that: The method for determining the filler height is: simulating the bending process of the wall panel with different filler heights through finite element simulation, when the stress peak in the finite element simulation result no longer changes with the filler height, the filler height at this time is the filler height to be determined.
4. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1 is characterized in that: The bending forming is performed by using a follow-up adjustable bending machine; The adjustable bending machine comprises an upper die set and a lower die set; The top of the upper die set is connected to the press, and the follower lower die set is located below the upper die set; the follower lower die set includes two lower die frames with adjustable spacing and a follower lower die installed on the lower die frame and capable of rotating relative to the lower die frame; The wall panel is placed between the upper die set and two follower lower dies; the wall panel is bent under the downward pressure applied by the upper die set, and the follower lower dies rotate accordingly.
5. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 4 is characterized in that: The bending forming process parameters include the bending force, which is calculated as follows: Π=W P -AT 弹 -AT 塑 ; Where Π is the total potential energy of the system; W P U is the work done by the bending force in the height direction of the sheet; 弹 is the elastic internal potential energy of the panel during the bending process; U 塑 is the internal potential energy of the panel during plastic deformation; The system uses a Cartesian coordinate system, where the x direction is the direction extending the rib length and parallel to the skin, the y direction is perpendicular to the rib elevation and parallel to the skin, and the z direction is perpendicular to the skin and parallel to the rib height. The origin of the coordinate system is set at the centroid of the bottom skin. Where D1 and D2 are the bending stiffness of the wall panel and filler, respectively. E1 and E2 are the Young's modulus of the wall plate and filler, respectively; t1 and t2 are the heights of the ribs and filler, respectively; ν1 and ν2 are the Poisson's ratios of the wall plate and filler, respectively; ω1 and ω2 are the deflection functions of the wall plate and filler, respectively, which are used to represent the displacement of the top of the rib after instability; The rib part of the panel is simplified to three-side fixed supports, and the deflection function of the panel is expressed as: The boundary conditions of the deflection function of the wall plate are: The packing part is simplified to three-side simply supported constraints, and the deflection function of the packing is expressed as: The boundary condition of the packing deflection function is: The grid of the wall panel is an oblique orthogonal grid, a is the length of the grid; b is the height of the wall panel; Where, P is the bending force; Let δΠ=0, take the minimum value Π min , the bending force is calculated.
6. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 5 is characterized in that: The bending forming process parameters also include the lower die spacing between the two follower lower dies, which is calculated as follows: In the formula, σ b is the tensile strength of the siding material; α is the arc of the lower die center; R is the bending radius of the siding; The curvature of the lower die center is calculated based on the bending force, and the lower die spacing is calculated based on the curvature of the lower die center.
7. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1 is characterized in that: The calculation method of the gap between the filler and the rib is as follows: using the axial mechanical balance model, a balance equation is established for the upper and lower sides of the neutral plane during the bending process of the wall panel: F b =F t =F 弹 +F 塑 ; In the formula, F b F is the tension in the lower part of the neutral layer; t is the pressure above the neutral layer; F 弹 is the compressive stress in the elastic deformation zone; F 塑 is the compressive stress in the plastic deformation zone; Where b1 is the height of the neutral layer; b s is the cut-off height of elastic deformation on one side of the neutral layer, ρ is the target curvature radius of the wall panel; σ s is the yield strength of the wallboard material; E1 and E2 are the Young's modulus of the wallboard and filler respectively; P is the compressive bending force; the grid of the wallboard is an oblique orthogonal grid, a is the length of the grid; b is the height of the wallboard; c is the thickness of the rib; t1 is the height of the rib; s0 is the gap between the filler and the rib; s1 is the height difference between the filler and the rib; Where N is the plastic strengthening modulus of the siding material; The gap between the filler and the ribs is calculated using the equilibrium equation.
8. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1 is characterized in that: The method for multi-pass bending and forming is: taking the center of the inner surface of the wall panel as a reference, drawing bending lines at equal intervals on both sides along the circumferential direction, and performing multi-pass progressive bending and forming according to the bending lines.
9. The multi-pass progressive bending forming method of the special material filled high-rib wall panel according to claim 1, characterized in that: The smooth surface of the meshed siding is covered with film and then filled with filler; After bending and forming, the wall panel is compared with the theoretical sample size of the inner surface and then pressurized point by point for correction.
10. The high-rib siding panel produced by the method according to any one of claims 1 to 9.
Citation Information
Cited By
Intelligent trial punching die and optimization method thereof
CN120460554A