Method for realizing clamp-free quick grinding and polishing of ceramic substrate

By fixing the ceramic substrate with paraffin wax and polishing it without fixtures on a single polishing machine, the problems of long fixture procurement cycle and high processing defect rate in the prior art are solved, realizing efficient and low-cost processing of ceramic substrates, which is suitable for a variety of product shapes.

CN118990318APending Publication Date: 2024-11-22SICHUAN LIUFANG YUCHENG ELECTRONIC TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410780975.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-18
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing ceramic substrate grinding and polishing technologies suffer from problems such as long fixture procurement cycles, high costs, high processing defect rates, low efficiency, and inability to process irregularly shaped products.

Method used

The ceramic substrate and ceramic disc were bonded together with paraffin wax. After being fixed by a hot press, they were polished without fixtures on a single polishing machine. The polishing pressure and speed were controlled to perform the process. After completion, the paraffin wax was removed by cleaning with anhydrous ethanol.

Benefits of technology

It shortens the processing cycle, improves processing efficiency and pass rate, reduces defect rate, can process irregularly shaped products, and does not require special fixtures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990318A_ABST
    Figure CN118990318A_ABST
Patent Text Reader

Abstract

The invention provides a method for realizing clamp-free quick grinding and polishing of a ceramic substrate. The method comprises the following steps: S1, adhering the ceramic substrate to the surface of a ceramic disc by using paraffin; s2, dipping dust-free cloth in absolute ethyl alcohol, and wiping to remove redundant paraffin on the surface of the ceramic substrate; s3, placing the assembly of the ceramic plate and the ceramic substrate on a single polishing machine for single-side processing; and S4, after machining is completed, a combined part of the ceramic disc and the ceramic substrate is taken out of the single polishing machine to be disassembled, and the surface of the ceramic substrate is cleaned. The invention provides a method for realizing clamp-free rapid grinding and polishing of a ceramic substrate, a clamp related in a conventional grinding and polishing process and manufacturing cost of the clamp can be replaced, the processing period of a wandering star wheel is saved, and the time can be averagely shortened by 5 days; broken edges and unfilled corners can be reduced, and the machining qualification rate is increased. And the size specification of the product is not required, and the special-shaped product can be processed.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of ceramic processing, and in particular to a method for realizing fixture-free rapid grinding and polishing of a ceramic substrate. Background Art

[0002] The existing common ceramic substrate grinding and polishing technology uses a planetary wheel as a loading fixture to fix the ceramic substrate, and then processes the product surface through a grinding and polishing machine. The current common grinding and polishing technology has the following disadvantages:

[0003] 1. It is necessary to purchase customized fixtures such as planetary wheels. The fixtures and product dimensions are one-to-one. If there are multiple types of products, multiple sets of planetary wheels must be purchased for matching. The procurement cycle of planetary wheels is usually 5-8 days, with an average price of 40 yuan per piece, which has a certain impact on the processing cycle and cost.

[0004] 2. There are also processing technology defects in fixing the substrate by the planetary wheel. In the fixture design, the slot of the planetary wheel must be larger than the outer dimensions of the substrate, usually 0.3mm (for example, if the processed product is 50.8*50.8mm, the sheet placement slot of the planetary wheel must be at least 51.1*51.1mm), so as to ensure that the substrate can be smoothly placed in the planetary wheel. However, due to the existence of the matching gap, the pressure and speed applied by the equipment to the product during the grinding and polishing process will cause the product to shake and collide in the planetary wheel. Therefore, if the processing parameters cannot be controlled well, the product will often have defects such as broken edges and missing corners. The greater the processing pressure and the higher the processing speed, the greater the defect rate of this type of defect will be, and even fragments and blown discs will occur.

[0005] 3. During the processing, the planetary wheel will also be subjected to pressure and rotational force by the equipment, and it will jump slightly in the equipment. This process will cause the planetary wheel to absorb part of the pressure, reducing the effective pressure on the product, and the direct result is a reduction in processing efficiency.

[0006] 4. In some special cases, such as special-shaped substrates, which do not have fixed length and width dimensions, it is impossible to design a planetary wheel for clamping, so grinding and polishing cannot be performed. Summary of the invention

[0007] In order to solve the technical problems existing in the above-mentioned background technology, the present invention provides a method for realizing fast grinding and polishing of a ceramic substrate without a fixture.

[0008] The present invention provides a method for realizing fixture-free rapid grinding and polishing of a ceramic substrate, comprising the following steps:

[0009] Step S1, sticking the ceramic substrate to the surface of the ceramic plate with paraffin;

[0010] Step S2, dampen a dust-free cloth with anhydrous ethanol and wipe away excess paraffin on the surface of the ceramic substrate;

[0011] Step S3, placing the assembly of the ceramic plate and the ceramic substrate on a single-sided polishing machine for single-sided processing;

[0012] Step S4: After the processing is completed, the assembly of the ceramic disc and the ceramic substrate is taken out from the single polishing machine for disassembly, and the surface of the ceramic substrate is cleaned.

[0013] In some embodiments, step S1 specifically includes:

[0014] Heat the paraffin at 115°C for 10 min to completely liquefy the paraffin, and then evenly apply it on the surface of the ceramic substrate;

[0015] Put the ceramic substrate on the surface of the ceramic plate, and use a hot press to apply 5MPa of pressure for 5 minutes to spread the paraffin evenly on the bonding surface in a hot melt state;

[0016] After naturally cooling to room temperature for 10 minutes, the ceramic substrate and the ceramic plate are completely fixed.

[0017] In some embodiments, in step S3, the polishing pressure is 4.65 g / mm2, the rotation speed is 35 rpm, and the time is 20 min.

[0018] In some embodiments, in step S4, the assembly is taken out, placed on a heating table and heated at 115° C. for 10 minutes to dissolve the paraffin, then the ceramic substrate is taken out and the liquid paraffin is cleaned with anhydrous ethanol, and finally the surface of the ceramic substrate is cleaned with a cleaning agent.

[0019] The beneficial effects of the present invention are:

[0020] The present invention provides a method for realizing fast grinding and polishing of ceramic substrates without fixtures, which can replace the fixtures and their manufacturing costs involved in conventional grinding and polishing processes, save the processing cycle of the planetary wheel, and can shorten the time by 5 days on average; improve the grinding and polishing efficiency, under the condition of meeting the same roughness requirements, the processing time of the new process is 20 minutes, and the conventional processing time is 30 minutes, which is shortened by 10 minutes; it can reduce edge collapse and corner chipping defects and improve the processing qualification rate. The conventional process test defect rate reaches 18%, while the new process reduces the processing defect rate to 0% within a reasonable parameter range; there is no requirement for the size specifications of the product, and the processing of special-shaped products can be realized. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] Figure 1 It is a schematic diagram of the processing structure of the present invention;

[0022] Figure 2 It is a schematic diagram of the processed product of the present invention. DETAILED DESCRIPTION

[0023] The following is a description of exemplary embodiments of the present disclosure in conjunction with the accompanying drawings, including various details of the embodiments of the present disclosure to facilitate understanding, which should be considered as merely exemplary. Therefore, it should be recognized by those of ordinary skill in the art that various changes and modifications may be made to the embodiments described herein without departing from the scope and spirit of the present disclosure. Similarly, for the sake of clarity and conciseness, descriptions of well-known functions and structures are omitted in the following description.

[0024] like Figure 1-2 As shown, an embodiment of the present invention discloses a method for realizing fixture-free rapid grinding and polishing of a ceramic substrate, comprising the following steps:

[0025] Step S1, sticking the ceramic substrate to the surface of the ceramic plate with paraffin;

[0026] Step S2, dampen a dust-free cloth with anhydrous ethanol and wipe away excess paraffin on the surface of the ceramic substrate;

[0027] Step S3, placing the assembly of the ceramic plate and the ceramic substrate on a single-sided polishing machine for single-sided processing;

[0028] Step S4: After the processing is completed, the assembly of the ceramic disc and the ceramic substrate is taken out from the single polishing machine for disassembly, and the surface of the ceramic substrate is cleaned.

[0029] In step S1, it specifically includes:

[0030] Heat the paraffin at 115°C for 10 min to completely liquefy the paraffin, and then evenly apply it on the surface of the ceramic substrate;

[0031] Put the ceramic substrate on the surface of the ceramic plate, and use a hot press to apply 5MPa of pressure for 5 minutes to spread the paraffin evenly on the bonding surface in a hot melt state;

[0032] After naturally cooling to room temperature for 10 minutes, the ceramic substrate and the ceramic plate are completely fixed.

[0033] In step S3, the polishing pressure is 3.88 g / mm2, the rotation speed is 30 rpm, and the time is 30 min.

[0034] In step S4, the assembly is taken out, placed on a heating table and heated at 115° C. for 10 minutes to dissolve the paraffin, and then the ceramic substrate is taken out and the liquid paraffin is cleaned with anhydrous ethanol. Finally, the surface of the ceramic substrate is cleaned with a cleaning agent.

[0035] Test example

[0036] A. Use the existing process to process 100 pieces of products for testing. Table 1 shows the standard process parameters:

[0037] Table 1

[0038] <![CDATA[Pressure g / mm 2 > Speed ​​rpm Time min Remark 3.88 30 30 Standard process parameters

[0039] After processing, the surface roughness can reach less than 30nm.

[0040] 100 pieces were processed and 10 pieces were randomly sampled for surface roughness. The results are shown in Table 2:

[0041] Table 2

[0042]

[0043] The 100 pieces were fully inspected and 82 pieces were found to be qualified. The specific defective conditions are shown in Table 3:

[0044] Table 3

[0045] fragments crack Collapse Missing corner Roughness is unqualified 2 5 6 4 1

[0046] B. Using the method disclosed in the present invention, 100 products were processed for testing. The polishing pressure was set to 3.88g / mm2, the speed was set to 30rpm, and the time was 30min. The test results showed that the surface roughness of the sampled products was less than 30nm; the number of broken edges and missing corners in the full inspection was 0, which met the qualified standard. The specific data of roughness are shown in Table 4:

[0047] Table 4

[0048]

[0049] The above test results show that the use of the new grinding and polishing method in combination with conventional process parameters can achieve a higher yield with equal efficiency, without chipping and corner problems, and with better surface roughness.

[0050] C. To improve the processing efficiency, the pressure was set to 4.65g / mm2 and the speed was set to 35rpm. The one-time processing time was shortened to 15min. 100 pieces were processed and the surface roughness of 10 pieces was randomly inspected. The test results are shown in Table 5:

[0051] Table 5

[0052]

[0053] The product roughness was 35-45nm, which was unqualified, but no abnormalities such as edge collapse and corner chipping were found. Therefore, the processing time was extended by 5 minutes and the inspection was repeated. The sampling results are shown in Table 6:

[0054] Table 6

[0055]

[0056] The product roughness is less than 30nm; the defective ratio of edge collapse and corner chipping is 0%, which meets the qualified standards.

[0057] Through this process method, the single-wheel processing time was shortened from the original 30 minutes to 20 minutes, a decrease of 10 minutes, and the defect rate of chipped edges and corners was reduced from the original 18% to 0%, thus successfully improving the grinding and polishing efficiency and yield.

[0058] D. Continue to improve the processing efficiency, set the pressure to 5g / mm2, the speed to 40rpm, and shorten the one-time processing time to 15min. 100 pieces were processed, 90 pieces were qualified, and the specific undesirable conditions are shown in Table 7:

[0059] Table 7

[0060] fragments crack 3 7

[0061] The surface roughness of 10 products sampled was found to be qualified, and the results are shown in Table 8:

[0062] Table 8

[0063]

[0064] The results show that using too high a pressure and rotation speed will cause material damage, so the process parameters of group C are the most reasonable.

[0065] For another part of irregular shaped products, the same conditions were used: heating at 115℃ for 10min, pressurizing at 5MPa for 5min, and cooling naturally to room temperature for 10min. The processing parameters were set to 4.65g / mm2, 35rpm, and 20min for one-time processing time, referring to the data of group C.

[0066] Without a fixture, 10 pieces of special-shaped products were polished. The surface roughness, thickness uniformity and appearance all met the requirements. The number of appearance defects such as broken edges and corners was 0. The inspection data is shown in Table 9:

[0067] Table 9

[0068]

[0069] Through this process, grinding and polishing of special-shaped products is successfully achieved, and the yield rate is consistent with that of standard products.

[0070] The above specific implementations do not constitute a limitation on the protection scope of the present disclosure. It should be understood by those skilled in the art that various modifications, combinations, sub-combinations and substitutions can be made according to design requirements and other factors. Any modification, equivalent substitution and improvement made within the spirit and principle of the present disclosure shall be included in the protection scope of the present disclosure.

Claims

1. A method for realizing fast grinding and polishing of ceramic substrate without fixture, characterized in that: The following steps are involved: Step S1, sticking the ceramic substrate to the surface of the ceramic plate with paraffin; Step S2, dampen a dust-free cloth with anhydrous ethanol and wipe away excess paraffin on the surface of the ceramic substrate; Step S3, placing the assembly of the ceramic plate and the ceramic substrate on a single-sided polishing machine for single-sided processing; Step S4: After the processing is completed, the assembly of the ceramic disc and the ceramic substrate is taken out from the single polishing machine for disassembly, and the surface of the ceramic substrate is cleaned.

2. A method for realizing fixture-free rapid grinding and polishing of a ceramic substrate according to claim 1, characterized in that: In step S1, it specifically includes: Heat the paraffin at 115°C for 10 min to completely liquefy the paraffin, and then evenly apply it on the surface of the ceramic substrate; Put the ceramic substrate on the surface of the ceramic plate, and use a hot press to apply 5MPa of pressure for 5 minutes to spread the paraffin evenly on the bonding surface in a hot melt state; After naturally cooling to room temperature for 10 minutes, the ceramic substrate and the ceramic plate are completely fixed.

3. The method for realizing fixture-free rapid grinding and polishing of a ceramic substrate according to claim 1, characterized in that: In step S3, the polishing pressure is 4.65 g / mm2, the rotation speed is 35 rpm, and the time is 20 min.

4. The method for realizing fixture-free rapid grinding and polishing of a ceramic substrate according to claim 1, characterized in that: In step S4, the assembly is taken out, placed on a heating table and heated at 115° C. for 10 minutes to dissolve the paraffin, then the ceramic substrate is taken out and the liquid paraffin is cleaned with anhydrous ethanol, and finally the surface of the ceramic substrate is cleaned with a cleaning agent.

Citation Information

Patent Citations

  • Polishing processing method for ultrathin sapphire wafer

    CN103639877A

  • Processing technique of ultrathin ceramic fingerprint identification pieces

    CN108237442A

  • Bonding method of light-emitting diode epitaxial wafer

    CN113658904A

  • High-efficiency single-side polishing method

    CN117067076A

  • Thin film circuit ceramic single-face grinding method