Prefabricated concrete component and preparation method thereof

By using retarded slurry and plastic film layer structure without aggregate in the preparation of concrete prefabricated components, the problem of cracking during the shrinkage process of concrete prefabricated components is solved, and the effect of reducing cracking risks and simplifying construction is achieved, avoiding the Use of fiber clumps and high admixtures.

CN118990734APending Publication Date: 2024-11-22CHINA STATE CONSTRUCTION ACADEMY CORPERATION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410883922.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-03
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Prefabricated concrete components are prone to cracks during shrinkage, which affects their anti-seepage, frost and chemical media erosion resistance. The existing technology such as adding fibers or adjusting the water-cement ratio has limitations, making it difficult to effectively reduce the risk of cracking.

Method used

Adopt a retarded slurry and plastic film layer structure without aggregate. The initial set time of retarded slurry is longer than that of structural concrete, reducing friction between the structural concrete layer and the mold, reducing shrinkage constraints, and combining an appropriate amount of retarder and powder Fly ash ensures free shrinkage during the plastic shrinkage stage and avoids cracking.

Benefits of technology

The risk of shrinkage and cracking of concrete prefabricated components is significantly reduced, and the theoretical crack resistance index is in the non-cracking or probabilistic cracking interval, avoids the use of fiber clumps and high admixtures, simplifies the construction process, and reduces costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118990734A_ABST
    Figure CN118990734A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of building material engineering, and particularly relates to a precast concrete component and a preparation method thereof. The preparation method comprises the following steps: 1) preparing a mold, and paving a first plastic film at the bottom of the mold; (2) delayed coagulation neat paste is injected into the mold paved with the first plastic film, and the delayed coagulation neat paste contains water, a cementing material and a retarder and does not contain aggregate; (3) paving a second plastic film on the surface of the delayed coagulation neat paste after the delayed coagulation neat paste is uniformly and flatly paved in the mold; and 4) injecting concrete into the mold paved with the second plastic film, further curing, and demolding to obtain the concrete. According to the present invention, by significantly reducing the constraint of the cement-based material and the mold, the shrinkage cracking risk during the concrete prefabricated member preparation process is substantially reduced, the theoretical anti-cracking index K is in the probabilistic cracking interval or the non-cracking interval, and the test result shows that the prepared concrete prefabricated member does not crack.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building material engineering, and in particular relates to a prefabricated concrete component and a preparation method thereof. Background Art

[0002] Prefabricated cement-based structures play an irreplaceable role in the development of building industrialization. The development trend of prefabricated concrete components in prefabricated buildings, decorative panels, road paving, bridge components, tunnel components, water conservancy project components, etc. continues to increase.

[0003] However, due to improper maintenance, chemical shrinkage or temperature shrinkage, cracks are prone to form on the surface of the components, or even through cracks, which not only affect the apparent quality of the components, but also the cracks in the plastic stage will remain until the hardening stage, allowing harmful substances to enter the matrix, seriously affecting the cement-based materials' impermeability, anti-freeze, resistance to chemical media erosion, and resistance to steel corrosion, and increasing the economic cost of the component factory. At present, many scholars have proposed various methods for reducing cracks in cement-based materials, such as adding fibers, using plastic films, curing agents and other materials to reduce the evaporation rate of water, etc. However, if the fiber content is too high, the fluidity of the mortar will decrease, and if the fiber length is too long, it will be easy to bend, which will reduce the effective length of contact with the matrix, resulting in reduced adhesion with the matrix, and the crack reduction ability is limited.

[0004] Patent publication number CN113049791A discloses a method for reducing plastic shrinkage cracking of cement-based materials, and proposes to reduce plastic shrinkage cracking of cement-based materials or eliminate cracking by synergistically adjusting three parameters: water-cement ratio, aggregate-cement ratio, and constraint degree. The patent proposes that the constraint degree is calculated by formula (1):

[0005] Constraint degree = 1-plastic shrinkage rate under constraint state / plastic shrinkage rate under quasi-free state (1)

[0006] The plastic shrinkage cracking resistance index K of cement-based materials was proposed. In the paper "Expansion of the Early Warning Mechanism of Plastic Shrinkage Cracking of Cement-based Materials", a seven-dimensional constitutive equation about K was constructed by integrating seven factors affecting cracking (see formula (2)). The cracking condition of cement-based materials was determined by the K value. K>1.86 means no cracking; 0.95<K<1.86 means probability of cracking; K<0.95 means cracking.

[0007] K=28.2×0.00434 Wc ×1.30 Sc ×0.994 FA ×0.247 SP ×0.322 C ×1.79 d ×0.166 v (2)

[0008] Where Wc is the water-cement ratio, Sc is the mortar-sand ratio, FA is the mass fraction of fly ash (%), SP is the mass fraction of water reducer (%), C is the degree of constraint, d is the degree of stratification, and v is the water loss evaporation rate (kg / (m 2 h)). Summary of the invention

[0009] In view of the deficiencies in the prior art, the present invention provides a precast concrete component and a method for preparing the same, which greatly reduces the shrinkage cracking problem occurring during the preparation of the precast concrete component from the perspective of reducing constraints.

[0010] Specifically, the present invention provides the following technical solutions:

[0011] A method for preparing a precast concrete component comprises the following steps:

[0012] 1) preparing a mold and laying a first plastic film on the bottom of the mold;

[0013] 2) injecting a retarding slurry into the mold covered with the first plastic film, wherein the retarding slurry comprises water, a gelling material and a retarder, but does not comprise aggregate;

[0014] 3) After the slow-setting slurry is evenly spread in the mold, a second plastic film is laid on the surface of the slow-setting slurry;

[0015] 4) injecting concrete into the mold covered with the second plastic film, further curing and demoulding, and thus obtaining the crack-reduced concrete prefabricated component.

[0016] The present invention arranges a slow-setting slurry without aggregate (sand and stone) between the mold and the concrete. Due to the plastic shrinkage stage, the initial setting time of the slow-setting slurry is longer than that of the structural concrete, and therefore no obvious constraint is exerted on the structural concrete layer. The friction between the structural concrete layer and the bottom mold is reduced, thereby reducing the risk of cracking of the structural concrete during the shrinkage process due to the inability to shrink freely due to the constraint of the bottom mold.

[0017] The slow-setting slurry used in the present invention is different from the traditional concrete only in that no sand is added. The reason is that adding sand will make the fluidity of the slow-setting slurry worse on the one hand, and increase the friction between the structural concrete and the slow-setting layer on the other hand, increasing the constraint between the two. At the same time, a certain amount of retarder is added to ensure that the slow-setting time is greater than the initial setting time of the engineering cement-based material, ensuring that the structural layer is not constrained by the bottom mold before hardening (i.e., the plastic shrinkage stage).

[0018] The present invention arranges a first plastic film between the mold and the slow-setting pure slurry, aiming to prevent the wooden mold from absorbing moisture of the slow-setting pure slurry and shortening the initial setting time of the slow-setting pure slurry.

[0019] The invention arranges a second plastic film between the slow-setting pure paste and the concrete, in order to prevent the slow-setting pure paste layer from mixing with the concrete layer and affecting the performance of the structural concrete.

[0020] The present invention has no special limitation on concrete, and its raw materials include water, cementitious materials and aggregates, which are weighed, stirred and poured according to the common method of mortar.

[0021] Preferably, in step 2), the cementitious material in the slow-setting slurry is made of the same material as the cementitious material in the concrete;

[0022] The water-binder ratio of the retarding paste is the same as that of the concrete. Studies have shown that by using the retarding paste with the same proportion as the concrete, the retarding layer and the structural layer shrink substantially synchronously, further reducing the constraints on the concrete layer.

[0023] Preferably, in step 2), the retarder is selected from at least one of sucrose, sodium gluconate and tartaric acid, and the amount of the retarder added is 0.05%-0.3% based on the mass of the cementitious material in the retarding slurry. If the amount added is too low, the initial setting time is fast, which increases the constraint with the structural layer.

[0024] Preferably, the slow-setting paste and concrete further contain fly ash;

[0025] And / or, the retarding paste and concrete further contain a water reducing agent. Studies have found that adding an appropriate amount of fly ash and a water reducing agent can reduce the risk of cracking of the concrete layer.

[0026] Preferably, in step 3), the thickness of the slow-setting slurry evenly spread in the mold is 2 mm or more, more preferably 2 to 3 mm. Studies have shown that when the thickness is less than 2 mm, uneven spreading occurs, which does not reduce the constraint effect.

[0027] Preferably, in step 1), the thickness of the first plastic film is 0.02-0.1 mm, and the material of the first plastic film is selected from at least one of CPP, hard PVC, and PE.

[0028] Preferably, in step 3), the thickness of the second plastic film is 0.02-0.1 mm, and the material of the second plastic film is selected from at least one of CPP, hard PVC, and PE.

[0029] Preferably, in step 4), the curing temperature is 10-20°C and the humidity is 60%-100%. Too high temperature and too low humidity will increase water evaporation and increase the risk of cracking.

[0030] The present invention provides a prefabricated concrete component, which is prepared by the above-mentioned preparation method. The prefabricated concrete component provided by the present invention can be widely used as an assembled prefabricated component, a curtain wall prefabricated board, and a cement-based material component board.

[0031] The beneficial effects of the present invention are at least:

[0032] (1) The method for preparing a precast concrete component provided by the present invention significantly reduces the constraints between concrete and the mold, thereby greatly reducing the risk of shrinkage cracking in the process of preparing the precast concrete component. The theoretical crack resistance index K is in the probability cracking range or the non-cracking range. The test results also show that the prepared concrete component does not crack.

[0033] (2) The method for preparing a precast concrete component provided by the present invention can replace the traditional method for preparing a precast concrete component by adding fibers to reduce cracking, or reduce other expensive admixtures such as shrinkage reducers and expansion agents, thereby greatly reducing costs. At the same time, it can avoid engineering problems such as fiber agglomeration, and the construction is simple and convenient.

[0034] (3) In the method for preparing a precast concrete component provided by the present invention, it is preferred that the cementitious material in the retarding slurry is of the same material as the cementitious material in the concrete, the water-binder ratio of the retarding slurry is the same as the water-binder ratio of the concrete, and the retarding layer and the structural layer shrink substantially synchronously, thereby further reducing the constraints on the concrete layer;

[0035] (4) In the method for preparing precast concrete components provided by the present invention, the retarding slurry and concrete preferably also contain fly ash and a water reducing agent. Studies have found that adding an appropriate amount of fly ash and a water reducing agent can reduce the risk of cracking of the concrete layer. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 This is a schematic diagram of the method for preparing a precast concrete component provided in Example 1; wherein 1 is concrete, 2 is a second plastic film, 3 is a first plastic film, 4 is a slow-setting slurry, and 5 is a mold. DETAILED DESCRIPTION

[0037] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be clearly and completely described in conjunction with the drawings in the embodiments of the present invention. The following embodiments are used to illustrate the present invention, but are not intended to limit the scope of the present invention. If no specific technology or conditions are specified in the embodiments, the technology or conditions described in the literature in the field or the product manual shall be followed.

[0038] Example 1

[0039] Example 1 provides a method for preparing a precast concrete component. Figure 1, including the following steps:

[0040] 1) Prepare a mold 5, and lay a first plastic film 3 (made of PE, with a thickness of 0.02 mm) on the bottom of the mold 5;

[0041] 2) injecting a slow-setting slurry 4 into the mold 5 covered with the first plastic film 3, wherein the slow-setting slurry 4 is composed of 2 parts by weight of water, 4 parts by weight of a gelling material (made of cement) and 0.008 parts by weight of a retarder (made of sucrose);

[0042] 3) After the slow-setting slurry 4 is evenly spread in the mold with a thickness of 2 mm, a second plastic film 2 (made of PE and with a thickness of 0.02 mm) is spread on the surface of the slow-setting slurry 4;

[0043] 4) injecting concrete 1 with a thickness of 20 mm into the mold 5 covered with the second plastic film 2, wherein the concrete 1 consists of 20 parts by weight of water, 40 parts by weight of cementitious material, and 40 parts by weight of aggregate (specifically, washed river sand with a fineness modulus of 2.7), curing for 24 hours in an environment of temperature 20° C. and humidity 75%, and demolding to obtain a precast concrete component.

[0044] Example 2

[0045] Embodiment 2 provides a method for preparing a precast concrete component, comprising the following steps:

[0046] 1) preparing a mold, and laying a first plastic film (made of PE, with a thickness of 0.02 mm) on the bottom of the mold;

[0047] 2) injecting a slow-setting slurry into the mold covered with the first plastic film, wherein the slow-setting slurry is composed of 1.6 parts by weight of water, 4 parts by weight of a gelling material (specifically cement), 0.008 parts by weight of a retarder (specifically sucrose), and 0.012 parts by weight of a water reducing agent (specifically a polycarboxylic acid-based water reducing agent);

[0048] 3) After the slow-setting slurry is evenly spread in the mold with a thickness of 2 mm, a second plastic film (made of PE and with a thickness of 0.02 mm) is spread on the surface of the slow-setting slurry;

[0049] 4) injecting concrete with a thickness of 20 mm into the mold covered with the second plastic film, wherein the concrete composition comprises 16 parts by weight of water, 40 parts by weight of cementitious material, 36 parts by weight of aggregate (specifically, washed river sand with a fineness modulus of 2.7) and 0.12 parts by weight of water reducer (specifically, polycarboxylic acid-based water reducer), curing for 24 hours in an environment of temperature 23° C. and humidity 65%, and demolding to obtain a precast concrete component.

[0050] Example 3

[0051] Embodiment 3 provides a method for preparing a precast concrete component, comprising the following steps:

[0052] 1) preparing a mold, and laying a first plastic film (made of PE, with a thickness of 0.02 mm) on the bottom of the mold;

[0053] 2) injecting a slow-setting slurry into the mold covered with the first plastic film, wherein the slow-setting slurry is composed of 2 parts by weight of water, 4 parts by weight of a gelling material (specifically, cement), and 0.008 parts by weight of a retarder (specifically, sucrose);

[0054] 3) After the slow-setting slurry is evenly spread in the mold with a thickness of 2 mm, a second plastic film (made of PE and with a thickness of 0.02 mm) is spread on the surface of the slow-setting slurry;

[0055] 4) injecting concrete with a thickness of 20 mm into the mold covered with the second plastic film, wherein the concrete composition comprises 20 parts by weight of water, 40 parts by weight of cementitious material, and 40 parts by weight of aggregate (specifically, washed river sand with a fineness modulus of 2.7), curing for 24 hours in an environment of temperature 27° C. and humidity 43%, and demolding to obtain a precast concrete component.

[0056] Example 4

[0057] Embodiment 1 provides a method for preparing a precast concrete component, comprising the following steps:

[0058] 1) preparing a mold, and laying a first plastic film (made of PE, with a thickness of 0.02 mm) on the bottom of the mold;

[0059] 2) injecting a slow-setting slurry into the mold covered with the first plastic film, wherein the slow-setting slurry comprises 2 parts by weight of water, 3.8 parts by weight of a gelling material (specifically cement and fly ash), 0.2 parts by weight of a gelling material (specifically cement and fly ash), and 0.008 parts by weight of a retarder (specifically sucrose);

[0060] 3) After the slow-setting slurry is evenly spread in the mold with a thickness of 2 mm, a second plastic film (made of PE and with a thickness of 0.02 mm) is spread on the surface of the slow-setting slurry;

[0061] 4) injecting concrete with a thickness of 20 mm into the mold covered with the second plastic film, wherein the concrete composition comprises 20 parts by weight of water, 38 parts by weight of cementitious material (specifically cement and fly ash), and 40 parts by weight of aggregate (specifically washed river sand with a fineness modulus of 2.7), curing for 24 hours in an environment of temperature 16° C. and humidity 80%, and demolding to obtain a precast concrete component.

[0062] Example 5

[0063] Embodiment 5 provides a method for preparing a precast concrete component, comprising the following steps:

[0064] 1) preparing a mold, and laying a first plastic film (made of PE, with a thickness of 0.02 mm) on the bottom of the mold;

[0065] 2) injecting a slow-setting slurry into the mold covered with the first plastic film, wherein the slow-setting slurry is composed of 2 parts by weight of water, 4 parts by weight of a gelling material (specifically, cement), and 0.008 parts by weight of a retarder (specifically, sodium gluconate);

[0066] 3) After the slow-setting slurry is evenly spread in the mold with a thickness of 2 mm, a second plastic film (made of PE and with a thickness of 0.02 mm) is spread on the surface of the slow-setting slurry;

[0067] 4) injecting concrete with a thickness of 20 mm into the mold covered with the second plastic film, wherein the concrete composition comprises 20 parts by weight of water, 40 parts by weight of a cementitious material (specifically cement), and 40 parts by weight of an aggregate (specifically washed river sand with a fineness modulus of 2.7), curing for 24 hours in an environment of a temperature of 28° C. and a humidity of 40%, and demolding to obtain a precast concrete component.

[0068] Compared with Example 3, the only difference in Example 5 is that sucrose in the retarding paste is replaced by sodium gluconate. Compared with sucrose, the retarding effect of sodium gluconate is not good, and the setting time is greatly shortened, so that the constraint between the structural concrete layer and the retarding paste is increased. The experimental results show that the constraint degree increases from 0.32 to 0.74.

[0069] Comparative Example 1

[0070] Comparative Example 1 adopts a conventional method for preparing a precast concrete component, comprising the following steps:

[0071] Prepare a mold, directly inject 20 mm thick concrete into the mold, the concrete composition is 20 parts by weight of water, 40 parts by weight of cementitious material, 40 parts by weight of aggregate (the material is specifically washed river sand with a fineness modulus of 2.7), cure for 24 hours in an environment of temperature 21° C. and humidity 78%, and demold, to obtain a precast concrete component.

[0072] Test example

[0073] The precast concrete components prepared in Examples 1-5 and Comparative Example 1 were subjected to performance tests, and the results are shown in Table 1.

[0074] Among them, the constraint degree was determined by the constraint degree test method in the paper “Study on the Constraint Parameters of Shrinkage Cracking of Cement-Based Materials and Hardening Crack Reduction”;

[0075] Substitute the parameters such as water-binder ratio, mortar-sand ratio, raw material dosage, constraint degree, stratification degree, water loss evaporation rate into formula (2) in patent CN 113049791A to calculate the theoretical anti-cracking index K value, and combine the test results to determine the crack reduction effect;

[0076] Table 1

[0077] Example 1 Example 2 Example 3 Example 4 Example 5 Comparative Example 1 Water-cement ratio 0.5 0.4 0.5 0.5 0.5 0.5 Mortar-sand ratio 1 1.1 1 1 1 1 Fly ash content / % 0 0 0 5 0 0 Water reducing agent dosage / % 0 0.3 0 0 0 0 <![CDATA[Water loss evaporation rate / (kg / (m 2 ·h)]]> 0.26 0.33 0.4 0.2 0.4 0.26 Constraint 0.32 0.32 0.32 0.32 0.74 0.94 Crack resistance index K 1.89 1.93 1.47 2.04 0.91 0.93 Test results No cracking No cracking No cracking No cracking Cracking Cracking

[0078] It can be seen from Table 1 that the preparation method of a precast concrete component proposed in the present invention can make the theoretical anti-cracking index K value greater than 0.95, which is in the non-cracking range or the probability cracking range. The test results are all non-cracking, which effectively reduces or even eliminates the cracking of cement-based materials, and provides a new idea and method for engineering crack reduction.

[0079] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A method for preparing a precast concrete component, characterized in that: The following steps are involved: 1) preparing a mold and laying a first plastic film on the bottom of the mold; 2) injecting a retarding slurry into the mold covered with the first plastic film, wherein the retarding slurry comprises water, a gelling material and a retarder, but does not comprise aggregate; 3) After the slow-setting slurry is evenly spread in the mold, a second plastic film is laid on the surface of the slow-setting slurry; 4) injecting concrete into the mold covered with the second plastic film, further curing and demoulding, and thus obtaining the crack-reduced concrete prefabricated component.

2. The method for preparing a precast concrete component according to claim 1, characterized in that: In step 2), the cementitious material in the slow-setting slurry is made of the same material as the cementitious material in the concrete; The water-to-binder ratio of the slow-setting paste is the same as that of the concrete.

3. A method for preparing a precast concrete component according to claim 1 or 2, characterized in that In step 2), the retarder is selected from at least one of sucrose, sodium gluconate and tartaric acid, and the amount of the retarder added is 0.05%-0.3% based on the mass of the gelling material in the retarding slurry.

4. A method for preparing a precast concrete component according to claim 1 or 2, characterized in that: The slow-setting paste and concrete also contain fly ash; And / or, the retarding paste and concrete further comprise a water reducing agent.

5. A method for preparing a precast concrete component according to claim 1 or 2, characterized in that: In step 3), the thickness of the slow-setting slurry evenly spread in the mold is greater than 2 mm.

6. A method for preparing a precast concrete component according to claim 1 or 2, characterized in that: In step 1), the thickness of the first plastic film is 0.02-0.1 mm, and the material of the first plastic film is selected from at least one of CPP, hard PVC, and PE.

7. A method for preparing a precast concrete component according to claim 1 or 2, characterized in that: In step 3), the thickness of the second plastic film is 0.02-0.1 mm, and the material of the second plastic film is selected from at least one of CPP, hard PVC, and PE.

8. A precast concrete component, characterized in that: It is prepared by the preparation method according to any one of claims 1 to 7.