Method for preparing AgSbTe2 nano material by solution method
AgSbTe2 nanomaterials were rapidly synthesized in oleamine solution by solution method, which solved the problems of high-temperature annealing and impurity phase generation in traditional methods, achieved low-cost and low-energy consumption large-scale production, and improved the thermoelectric performance and application value of the material.
Patent Information
- Application Number
- CN202411129802.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-16
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-16
AI Technical Summary
The prior art is difficult to rapidly synthesize high-performance AgSbTe2 nanomaterials on a large scale through solution methods, and traditional methods have problems such as high-temperature annealing, impurity phase generation and high cost, which limits the practical application of the materials.
The solution method is used to prepare AgSbTe2 nanomaterials. By adding molecular ligands of Ag and Sb to the oleamine solution, then rapidly warming up and adding Te source precursors, the reaction conditions are controlled to avoid the generation of impurities and achieve rapid synthesis at low temperature.
The large-scale rapid and precise synthesis of AgSbTe2 nanomaterials has been achieved, which reduces cost and energy consumption, avoids the generation of impurity phases, and significantly improves the thermoelectric performance and application value of the material.
Smart Images

Figure CN118992989A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of nano material preparation, and in particular to a method for preparing AgSbTe2 nano material by a solution process. Background Art
[0002] As a type of functional material, thermoelectric materials can directly convert temperature difference into electrical energy or use electrical energy to generate temperature difference refrigeration. They are widely used in energy recovery, refrigeration and sensing. These materials realize direct energy conversion through the thermoelectric effect. Their core performance index is the thermoelectric figure of merit (zT value, zT = σS2T / κ), which is a key indicator to measure the comprehensive performance of the material and reflects the relationship between the material's electrical conductivity (σ), Seebeck coefficient (S) and thermal conductivity (κ) (where T is the absolute temperature). With the increasing prominence of environmental problems and the continuous growth of energy demand, the development and optimization of high-performance thermoelectric materials, especially those that can work effectively at room temperature or medium temperature range, has become an important research direction in materials science. AgSbTe2 is a medium-temperature thermoelectric material. Its high thermoelectric figure of merit zT and good performance stability have attracted widespread attention from researchers. This material has shown high thermoelectric conversion efficiency in the medium temperature region, making it an ideal choice for thermoelectric power generation and refrigeration applications. The crystal structure of AgSbTe2 is a face-centered cubic structure, which helps optimize its electron transport performance while maintaining a low thermal conductivity κ, which is a key factor in improving thermoelectric performance. In addition, its application potential and optimization space in the field of thermoelectric materials still need to be further explored and developed, indicating the great application prospects of AgSbTe2 in the field of energy conversion materials.
[0003] Traditionally, the synthesis of AgSbTe2 mainly relies on solid-phase reaction and high-temperature melting method, especially vacuum melting method. Although these methods can achieve the preparation of AgSbTe2 to a certain extent, they face many challenges. In order to prevent the vacuum quartz tube from breaking due to rapid temperature changes, the melting method requires an extremely slow heating and cooling speed (about 0.3-0.4K·min) during the processing. -1 ), and requires extremely high temperatures above the melting point of its raw materials and maintained for a long time. In addition, in order to promote the formation of the main phase of AgSbTe2, this method also requires long-term low-temperature annealing, which may even last for several days. However, even with this slow and time-consuming process, the generation of impurity phases such as Ag2Te and Sb2Te3 cannot be avoided, and these impurity phases will significantly affect the thermoelectric transport properties of AgSbTe2 materials.
[0004] Since the size of the nanostructure is close to the mean free path of phonons, the thermal conductivity κ can be effectively further reduced by scattering phonons, thereby enhancing the thermoelectric figure of merit zT of the material. Therefore, in order to prepare AgSbTe2 nanostructured materials, some traditional preparation strategies other than vacuum melting have been adopted, such as chemical vapor transport, ultrasonic chemical preparation and solid phase reaction. Although they have their unique advantages, they generally have problems such as long preparation time, high cost, cumbersome process and high temperature annealing. So far, an effective strategy for directly preparing AgSbTe2 nanomaterials by solution synthesis has not been found. Typical liquid phase synthesis is mainly based on hydrothermal / solvothermal method with high pressure reactor as reaction vessel, which can prepare nano-scale composite materials, but its large-scale preparation is severely limited, reducing the economic feasibility of practical application. Therefore, the development of a new method that can achieve large-scale preparation at low temperature and accurately control the chemical composition and micromorphology is not only of great academic value, but also crucial to improving the practical application of thermoelectric materials. Summary of the invention
[0005] The purpose of the present invention is to provide a method for preparing AgSbTe2 nanomaterials by a solution process. The preparation method is simple, the synthesis conditions are mild and the energy consumption is low. It can achieve large-scale, rapid and accurate synthesis of AgSbTe2 nanomaterials with intrinsic low thermal conductivity, and has good practical application value.
[0006] In one aspect of the present invention, the present invention provides a method for preparing AgSbTe2 nanomaterials by a solution process. According to an embodiment of the present invention, the method comprises the following steps:
[0007] The molecular ligand solutions of Ag and Sb are respectively added to the preheated and vacuum degassed oleylamine solution, and the temperature is rapidly raised to a specific temperature under the protection of argon to obtain a cationic solution. The Te source precursor is injected into the above-mentioned reacted cationic solution and kept warm for a certain period of time. After the reaction solution is cooled to room temperature, centrifuged and washed to prepare AgSbTe2 nanocrystals.
[0008] In addition, the method for preparing AgSbTe2 nanomaterials by a solution method according to the above embodiment of the present invention may also have the following additional technical features:
[0009] In some embodiments of the present invention, the method specifically comprises the following steps:
[0010] (1) Preparation of anion and cation precursors
[0011] At room temperature, Te particles were dissolved in tri-n-octylphosphine in a glove box and stirred to prepare a Te source precursor;
[0012] At room temperature, in an argon atmosphere, Ag2O and Sb2O3 are added to a mixed solution of oleylamine and ethanethiol in a certain volume ratio, and stirred to prepare a molecular ligand solution of Ag and Sb, which is a cationic precursor;
[0013] (2) Preparation of AgSbTe2 nanomaterials by liquid phase method
[0014] After oleylamine is vacuum-degassed for a certain period of time under certain temperature conditions, argon is introduced, and cationic Ag and Sb molecular ligand solutions are injected into the oleylamine solvent at a molar ratio of 1: (0.98-1.02), and then the temperature is rapidly raised to change the solution from turbid light brown to transparent yellow, and then Te source precursor is added to react. After the reaction, centrifugal washing and vacuum drying are carried out to obtain AgSbTe2 nanomaterials.
[0015] In some embodiments of the present invention, in step (1), the concentration of the Te source precursor is 1.0 mol·L -1 The stirring time of Te particles and tri-n-octylphosphine is 3-5 days.
[0016] In some embodiments of the present invention, in step (1), the volume ratio of oleylamine to ethyl mercaptan is (3-4):1, and the stirring time is 6-12h.
[0017] In some embodiments of the present invention, in step (2), oleylamine is vacuum degassed for not less than 30 minutes at a temperature of 100-130°C.
[0018] In some embodiments of the present invention, in step (2), the molar ratio of Ag, Sb and Te is 1:(0.98-1.02):(2-2.05).
[0019] In some embodiments of the present invention, in step (2), the reaction temperature is 170-190° C., the reaction time is 50-70 min, and the washing is performed by centrifugal washing with n-hexane and anhydrous ethanol for 2-4 times.
[0020] In some embodiments of the present invention, in step (2), the centrifugal speed is 7000-9000 rpm, and the time is 5-10 min each time.
[0021] In some embodiments of the present invention, in step (2), the drying is performed by vacuum drying, the drying time is 4-8 hours, and the drying temperature is 60-80°C.
[0022] In another aspect of the present invention, the present invention provides an AgSbTe2 nanomaterial prepared according to the method for preparing AgSbTe2 nanomaterial by the solution method. According to an embodiment of the present invention, the AgSbTe2 nanomaterial has a NaCl cubic rock salt structure.
[0023] Compared with the prior art, the present invention has the following beneficial effects:
[0024] (1) The present invention is mainly devoted to the preparation of AgSbTe2 nanomaterials by solution method with controllable morphology and size, large quantities and low cost. Compared with the traditional solid phase vacuum melting method, the method of the present invention effectively solves the problem of Ag2Te and Sb2Te3 impurity phases that are difficult to eliminate during the melting process, and avoids the limitations of uncontrollable impurity phases, long cycles and high energy consumption.
[0025] (2) Existing chemical methods such as chemical vapor transport and ultrasonic chemical preparation can synthesize AgSbTe2, but the cost is high and the output is limited to the milligram level, and usually requires cumbersome post-annealing treatment to obtain the main phase. It has been reported that expensive and highly flammable lithium bis(trimethylsilylamide) (LiN(SiMe3)2) was used as a reducing agent for the pure phase synthesis of AgSbTe2 at the microgram level, but this greatly limits its practical application. The present invention uses relatively cheap oxides Ag2O and Sb2O3 as raw materials to prepare Ag and Sb molecular ligands as cationic precursors, which are then reacted with Te source precursors in molar ratios. Through a unique low-temperature rapid synthesis strategy, AgSbTe2 nanomaterials can be prepared on a large scale.
[0026] (3) The present invention not only significantly reduces the preparation cycle and cost, but also effectively avoids the inevitable generation of impurity phases during the cooling process in solid-phase synthesis. Compared with the traditional "top-down" solid-phase melting method, the low-temperature synthesis strategy of the present invention can more accurately control the interface morphology and size of the material, demonstrating the uniqueness and superiority of its technology. BRIEF DESCRIPTION OF THE DRAWINGS
[0027] Figure 1 The X-ray diffraction pattern (XRD) of the AgSbTe2 nanomaterial prepared in Example 1 of the present invention;
[0028] Figure 2 a) and b) are scanning electron microscope (SEM) images of the AgSbTe2 nanomaterial powder prepared in Example 1 of the present invention at different magnifications, wherein a) × 20.0K, b) × 30.0K;
[0029] Figure 3 TEM image of the AgSbTe2 nanomaterial prepared in Example 1 of the present invention, wherein Figure b) is an enlarged image of the area in the white frame in Figure a);
[0030] Figure 4The scanning transmission electron microscope (STEM) image of the AgSbTe2 nanomaterial prepared in Example 1 of the present invention and the element distribution map of the corresponding nanoparticles, a) high angle annular dark field (HAADF) image of the AgSbTe2 nanoparticles, b) Ag, the table in the figure is the EDX spectrum analysis in the scanning transmission electron microscope, that is, the atomic percentages of the three elements Ag, Sb and Te, c) Sb, d) Te;
[0031] Figure 5 The scanning transmission electron microscope (STEM) image of the AgSbTe2 nanomaterial prepared in Example 1 of the present invention and the element distribution map of the corresponding nanorods, a) high angle annular dark field (HAADF) image of the AgSbTe2 nanorods, b) Ag, the table in the figure is the EDX spectrum analysis in the scanning transmission electron microscope, that is, the atomic percentages of the three elements Ag, Sb and Te, c) Sb, d) Te;
[0032] Figure 6 The X-ray diffraction patterns (XRD) of the AgSbTe2 nanomaterials in Comparative Examples 1-4 and Example 1 of the present invention are shown. DETAILED DESCRIPTION
[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0034] Example 1
[0035] A method for preparing AgSbTe2 nanomaterials by a solution process comprises the following steps:
[0036] (1) Preparation of anion and cation precursors
[0037] a. Preparation of large quantities of anionic Te precursor: At room temperature, 50 mmol of Te particles were placed in a 50 mL glass container of tri-n-octylphosphine (TOP) in a glove box and magnetically stirred for 5 days until they were completely dissolved. Finally, the solution turned into a bright yellow clear solution. Finally, a 1.0 mol·L -1 Te source precursor (Te-TOP) stock solution.
[0038] b. Preparation of cationic precursors: First, 20 mL of oleylamine was vacuum degassed at 120°C for 60 min to remove low-boiling substances, and then argon was introduced. Second, 2.0 mmol of Ag2O and Sb2O3 powders were weighed in a glass bottle filled with argon, and added to a mixed solution of 8 mL of degassed oleylamine and 2 mL of ethanethiol, with a volume ratio of 4:1. The solution was stirred magnetically at room temperature for 12 h until it was completely clear and transparent. Finally, a 0.4 mol·L -1 Molecular ligand solutions of Ag and Sb.
[0039] (2) Preparation of AgSbTe2 nanomaterials by liquid phase method
[0040] c. First, 70 mL of oleylamine was degassed under vacuum at 120°C for 60 min to remove low-boiling substances, and then argon was introduced. Then, 0.4 mol·L -1 The molecular ligand solutions of cationic Ag and Sb were injected into the oleylamine solvent in a molar ratio of 1:1 (volume of each was 10 mL), and the temperature was rapidly raised under argon protection. During the process, the solution changed from a turbid light brown to a yellow transparent solution at about 170°C. When the temperature reached 180°C, 8 mL of 1.0 mol·L pre-prepared in step (1a) was added. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2. The reaction time was 60 minutes at 180°C and then cooled to room temperature in a water bath.
[0041] d. After the reaction is completed and cooled, the solution is centrifuged and washed with n-hexane as a dispersant and anhydrous ethanol as a precipitant. The volume ratio of n-hexane to anhydrous ethanol is 1:1. The centrifugal washing is performed 3 times at a speed of 9000 rpm for 5 minutes each time. Finally, the obtained AgSbTe2 nanoparticles are transferred to a vacuum drying oven and dried at 60°C for 6 hours. Finally, about 1.7g of AgSbTe2 nanomaterial powder can be obtained, and the yield is close to 90% of the theoretical yield.
[0042] like Figure 1 As shown, the XRD peaks of the AgSbTe2 nanomaterial prepared in Example 1 completely correspond to the diffraction peaks of the standard card (PDF#00-015-0540) of the AgSbTe2 material, proving that the liquid phase method used in the present invention successfully synthesized pure phase AgSbTe2. In addition, the samples synthesized in this patent have no obvious impurity phase, showing the significant advantage of its composition control.
[0043] like Figure 2As shown, the material morphology synthesized by the liquid phase method adopted in this embodiment is nanoparticles and nanorods. The size of the nanorods is tens of nanometers in width and 1-2 micrometers in length, and the size of the nanoparticles is about tens to hundreds of nanometers.
[0044] like Figure 3 As shown in the two TEM characterizations, the morphology and size of the prepared AgSbTe2 nanomaterials can be observed. Figure 2 The characterization results of scanning electron microscopy were consistent with those of nanoparticles and nanorods.
[0045] like Figure 4 As shown, the scanning transmission electron microscopy element distribution results show that: except for a smaller area where Ag is slightly enriched, the elements of Ag, Sb and Te are evenly distributed in other large areas, and the total atomic percentage is close to the stoichiometric ratio of 1:1:2.
[0046] like Figure 5 As shown, the scanning transmission electron microscopy element distribution results show that the three elements Ag, Sb and Te are evenly distributed on the surface of the nanorods, the Ag content inside the nanorods is relatively high, and the total atomic percentage is close to the stoichiometric ratio of 1:1:2.
[0047] Example 2
[0048] A method for preparing AgSbTe2 nanomaterials by a solution process comprises the following steps:
[0049] (1) Preparation of anion and cation precursors
[0050] a. Preparation of large amounts of anionic Te precursor: At room temperature, 50 mmol of Te particles were placed in a 50 mL glass container of tri-n-octylphosphine (TOP) in a glove box and stirred magnetically for 5 days until it was completely dissolved. Finally, the solution turned into a bright yellow clear solution. Finally, a 1.0 mol·L -1 Te source precursor (Te-TOP) stock solution.
[0051] b. First, 40 mL of oleylamine was vacuum degassed at 120°C for 60 min to remove the low-boiling substances, and then argon was introduced. Secondly, 4.0 mmol of Ag2O and Sb2O3 powders were weighed in a glass bottle filled with argon, and added to 16 mL of degassed oleylamine and 4 mL of ethanethiol mixed solution, with the volume ratio of oleylamine to ethanethiol being 4:1. The solution was stirred magnetically at room temperature for 12 h until it was completely clear and transparent. Finally, a 0.4 mol·L -1 Molecular ligand solutions of Ag and Sb.
[0052] (2) Liquid phase method for mass preparation of AgSbTe2 nanomaterials
[0053] c. First, 140 mL of oleylamine was degassed under vacuum at 120°C for 60 min to remove low-boiling substances, and then argon was introduced. Then, 0.4 mol·L -1 The molecular ligand solutions of cationic Ag and Sb were injected into the oleylamine in a molar ratio of 1:1 (volume of each was 20 mL), and the temperature was rapidly raised under argon protection. During the process, the solution changed from a turbid light brown to a yellow transparent solution at about 170°C. When the temperature reached 180°C, 16 mL of 1.0 mol·L pre-prepared in step (1a) was added. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2. The reaction time was 60 minutes at 180°C and then cooled to room temperature in a water bath.
[0054] d. After the reaction is completed and cooled, the solution is centrifuged and washed with n-hexane as a dispersant and anhydrous ethanol as a precipitant. The volume ratio of n-hexane to anhydrous ethanol is 1:1. The centrifugal washing is performed 3 times at a speed of 9000 rpm for 5 minutes each time. Finally, the obtained AgSbTe2 nanoparticles are transferred to a vacuum drying oven and dried at 60°C for 6 hours. The doubled reaction can finally obtain about 3.5g of AgSbTe2 nanomaterial powder, and the yield is also close to 90% of the theoretical yield.
[0055] Example 3
[0056] A method for preparing AgSbTe2 nanomaterials by a solution method. The difference between this embodiment and embodiment 1 is that in step d of embodiment 1, when the solution changes from turbid light brown to yellow transparent solution at 170°C, 8 mL of 1.0 mol·L pre-prepared in step 1a is added to the mixture. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2, and the reaction time was 60 minutes at 170°C, and then cooled to room temperature in a water bath. The remaining steps were the same as those in Example 1.
[0057] In the present invention, whether the multiple of the reactants is enlarged or reduced, it is effective to use oleylamine and ethyl mercaptan as solvents to prepare cationic molecular ligand precursors, and the volume ratio is set to 3-4. In addition, the degassing temperature of oleylamine is set at 100-130°C, the final reaction temperature is controlled at 170-190°C, and the reaction time is 50-70min. These parameter ranges can effectively implement the present invention. For the sake of brevity, all embodiments are no longer listed one by one. For specific situations where the present invention cannot be implemented, please refer to the comparative example section in the description to understand the relevant differences in raw materials and reaction conditions.
[0058] The comparative examples are set up to compare with the methods for preparing AgSbTe2 nanomaterials in Examples 1-3. The comparative examples cannot prepare pure phase AgSbTe2 nanomaterials. The present invention specifically lists 4 cases for illustration. All the anion precursors Te-TOP are consistent with the steps in Examples 1-3, mainly including the following steps:
[0059] Comparative Example 1
[0060] Step 1, preparation of anion and cation precursors, comprising the following steps:
[0061] a.1.0mol·L -1 The preparation of the anionic Te precursor is consistent with that of Example 1-3.
[0062] Step 2: Prepare AgSbTe2 nanomaterials by liquid phase method, comprising the following steps:
[0063] b. First, add 5mmol of AgNO3 and 5mmol of SbCl3 into a three-necked flask containing 70mL of oleylamine, stir magnetically at room temperature for 20min, evacuate and circulate argon for three times, then heat to 120℃ under vacuum for degassing for 60min to remove low-boiling substances, and then introduce argon. Then, when the temperature is quickly raised to 220℃, 10mL of Te source precursor Te-TOP prepared in step (1a) is injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2, and the reaction time is 60min at 220℃, and then cooled to room temperature in a water bath.
[0064] c. After the reaction is completed and the solution is cooled, the centrifugal washing and vacuum drying conditions are the same as those in Example 1-3.
[0065] Comparative Example 2
[0066] Step 1, preparation of anion and cation precursors, comprising the following steps:
[0067] a.1.0mol·L -1 The preparation of the anionic Te precursor is consistent with that of Example 1-3.
[0068] b.0.4mol·L -1 The preparation of the Ag and Sb molecular ligand solutions is consistent with that of Examples 1-3.
[0069] Step 2: Prepare AgSbTe2 nanomaterials by liquid phase method, comprising the following steps:
[0070] c. First, 70 mL of oleylamine was degassed under vacuum at 120°C for 60 min to remove the low-boiling substances therein, and then argon was introduced. Then, 0.4 mol·L -1 The molecular ligand solutions of cationic Ag and Sb were injected into the oleylamine in a molar ratio of 1:1 (volume of each was 10 mL), and the temperature was rapidly raised under argon protection. During the process, the solution changed from a turbid light brown to a yellow transparent solution at about 170°C. When the temperature reached 220°C, 8 mL of 1.0 mol·L pre-prepared in step (1a) was added. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2. The reaction time was 60 minutes at 220°C and then cooled to room temperature in a water bath.
[0071] d. After the reaction is completed and the solution is cooled, the centrifugal washing and vacuum drying conditions are the same as those in Example 1-3.
[0072] Comparative Example 3
[0073] Step 1, preparation of anion and cation precursors, comprising the following steps:
[0074] a.1.0mol·L -1 The preparation of the anionic Te precursor is consistent with that of Example 1-3.
[0075] b. First, 20 mL of oleylamine was vacuum degassed at 120°C for 60 min to remove the low-boiling substances, and then argon was introduced. Secondly, 2.0 mmol of Ag2O and Sb2O3 powders were weighed in a glass bottle filled with argon, and added to a mixed solution of 8 mL of degassed oleylamine and 2 mL of ethanedithiol, with a volume ratio of 4:1. The solution was stirred magnetically at room temperature for 12 h until it was completely clear and transparent. Finally, a 0.4 mol·L -1 Molecular ligand solutions of Ag and Sb.
[0076] Step 2: Prepare AgSbTe2 nanomaterials by liquid phase method, comprising the following steps:
[0077] c. First, 70 mL of oleylamine was degassed under vacuum at 120°C for 60 min to remove the low-boiling substances therein, and then argon was introduced. Then, 0.4 mol·L -1The molecular ligand solutions of cationic Ag and Sb were injected into the oleylamine in a molar ratio of 1:1 (volume of each was 10 mL), and the temperature was rapidly raised under argon protection. During the process, the solution changed from a turbid light brown to a yellow transparent solution at about 170°C. When the temperature reached 180°C, 8 mL of 1.0 mol·L pre-prepared in step (1a) was added. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2. The reaction time was 60 minutes at 180°C and then cooled to room temperature in a water bath.
[0078] d. After the reaction is completed and the solution is cooled, the centrifugal washing and vacuum drying conditions are the same as those in Example 1-3.
[0079] Comparative Example 4
[0080] Step 1, preparation of anion and cation precursors, comprising the following steps:
[0081] a.1.0mol·L -1 The preparation of the anionic Te precursor is consistent with that of Example 1-3.
[0082] b.0.4mol·L -1 The preparation of the Ag and Sb molecular ligand solutions is consistent with that of Examples 1-3.
[0083] Step 2: Prepare AgSbTe2 nanomaterials by liquid phase method, comprising the following steps:
[0084] c. First, 70 mL of oleylamine was degassed under vacuum at 120°C for 60 min to remove the low-boiling substances therein, and then argon was introduced. Then, 0.4 mol·L -1 The molecular ligand solutions of cationic Ag and Sb were injected into the oleylamine in a 1:1 molar ratio (volume of each was 10 mL), and the temperature was rapidly raised under argon protection. During the process, the solution changed from a turbid light brown to a yellow transparent solution at about 170°C. When the temperature reached 180°C, 8 mL of 1.0 mol·L pre-prepared in step (1a) was added. -1 The Te source precursor Te-TOP was injected into the cationic solution of Ag and Sb according to the molar ratio of Ag, Sb and Te of 1:1:2. The reaction time was 180 minutes at 180°C and then cooled to room temperature in a water bath.
[0085] d. After the reaction is completed and the solution is cooled, the centrifugal washing and vacuum drying conditions are the same as those in Example 1-3.
[0086] Through detailed analysis of Examples 1-3 and Comparative Examples 1-4, combined with Figure 6The X-ray diffraction (XRD) results are shown in Table 1. Table 1 shows the corresponding products of Examples 1-3 and Comparative Examples 1-4. The table lists the implementation parameters and reaction conditions in detail, and clarifies the corresponding relationship between the products of each example and comparative example. All anion precursors in the examples and comparative examples are at a concentration of 1.0 mol·L -1 The concentrations of Te-TOP, Ag and Sb cation precursors were all 0.4 mol·L -1 , the reaction solvents are all oleylamine, so they are not listed in this table. The difference between Example 2 and Example 1 in the table is that it is a reaction with an enlarged multiple, in which the prepared products of Comparative Examples 1-4 in the table are arranged in the order of main phase and secondary phase. In the table, OLA represents oleylamine, EtSH represents ethanethiol, and EDT represents ethanedithiol.
[0087] Table 1 Results of the products prepared by Examples 1-3 and Comparative Examples 1-4
[0088]
[0089] like Figure 6 As shown, the obtained in Comparative Examples 1-4 all contain Ag2Te and Sb2Te3 impurity phases. Specifically, in Comparative Example 1, in addition to the peak of the main phase AgSbTe2, it also contains obvious Ag2Te phase and Sb2Te3 phase; while in Comparative Example 2, the main phase is mainly Ag2Te phase and Sb2Te3 phase, and the peak of AgSbTe2 is extremely low; in Comparative Example 3, the main phase is Sb2Te3 phase, and the content of Ag2Te phase and AgSbTe2 phase is low; in Comparative Example 4, the main phase is Sb2Te3 phase and AgSbTe2 phase, and it also contains a small amount of Ag2Te phase; the preparation result of Example 1 is pure phase AgSbTe2.
[0090] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the structure of the present invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.
Claims
1. Preparation of AgSbTe by a solution method 2 Nanomaterials methods, It is characterized in that The following steps are involved: The molecular ligand solutions of Ag and Sb were added to the preheated and vacuum degassed oleylamine solution, and the temperature was rapidly raised to a specific temperature under the protection of argon to obtain a cationic solution. The Te source precursor was injected into the above-mentioned reacted cationic solution and kept warm for a certain period of time. After the reaction was completed, the reaction solution was cooled to room temperature and centrifuged and washed to prepare AgSbTe. 2 Nanocrystals.
2. Preparation of AgSbTe by a solution method according to claim 1 2 Nanomaterials methods, It is characterized in that The steps include: (1) Preparation of anion and cation precursors At room temperature, Te particles were dissolved in tri-n-octylphosphine in a glove box and stirred to prepare a Te source precursor; At room temperature, in an argon atmosphere, Ag 2 O and Sb 2 O 3 Add them to a mixed solution of oleylamine and ethanethiol in a certain volume ratio, stir and prepare a molecular ligand solution of Ag and Sb, which is a cationic precursor; (2) Liquid phase method for preparing AgSbTe 2 Nanomaterials After oleylamine is vacuum-degassed for a certain period of time under certain temperature conditions, argon is introduced, and the cationic Ag and Sb molecular ligand solutions are injected into the oleylamine solvent at a molar ratio of 1: (0.98-1.02), and then the temperature is rapidly raised to change the solution from turbid light brown to yellow transparent, and then Te source precursor is added to react. After the reaction is completed, centrifugal washing and vacuum drying are performed to obtain AgSbTe 2 Nanomaterials.
3. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In step (1), the concentration of the Te source precursor is 1.0-2.0 mol·L -1 The stirring time of Te particles and tri-n-octylphosphine is 3-5 days.
4. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (1), the volume ratio of oleylamine to ethanethiol is (3-4):1, and the stirring time is 6-12h.
5. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (2), oleylamine is vacuum degassed for no less than 30 minutes at a temperature of 100-130°C.
6. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (2), the molar ratio of Ag, Sb and Te is 1:(0.98-1.02):(2-2.05).
7. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (2), the reaction temperature is 170-190° C., the reaction time is 50-70 min, and the washing is performed by centrifugal washing with n-hexane and anhydrous ethanol for 2-4 times.
8. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (2), the centrifugal speed is 7000-9000 rpm, and the time is 5-10 minutes each time.
9. Preparation of AgSbTe by a solution method according to claim 2 2 Nanomaterials methods, Features: In the step (2), vacuum drying is used for drying, the drying time is 4-8 hours, and the drying temperature is 60-80°C.
10. A solution method for preparing AgSbTe according to any one of claims 1 to 9 2 Single-phase AgSbTe prepared by nanomaterial method 2 Nanocrystals, Features: The single-phase AgSbTe 2 The nanocrystals have a NaCl cubic rock salt structure.
Citation Information
Patent Citations
Sonochemistry method for preparing AgSbTe2 thermoelectric compound powder
CN101602494A
Method for synthesizing CdTe nano-rods in organic phase
CN104386656A
Rhombic phase SnSb2Te4 nano material and preparation method and application thereof
CN118183636A