Biological matrix hard carbon sodium ion battery negative electrode material and preparation method thereof

By using coconut shell as a precursor and combining high-temperature heat treatment and sulfur doping processes, a bio-based hard carbon sodium-ion battery anode material was prepared, solving the problems of high cost and environmental pollution of sodium-ion battery anode materials, and achieving high reversible capacity and excellent cycle performance.

CN118993028APending Publication Date: 2024-11-22JIANGXI ZHENGTUO NEW ENERGY TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411113353.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

There is a lack of suitable anode materials for existing sodium-ion batteries, and existing anode materials are expensive and cause environmental pollution problems.

Method used

Using coconut shells, which have low impurity content and high strength, as a precursor, the pore structure, surface oxygen-containing functional groups, and graphite microcrystalline structure of biomass hard carbon are controlled through high-temperature heat treatment and sulfur doping processes to prepare a bio-based hard carbon sodium-ion battery anode material.

Benefits of technology

It significantly improves the reversible capacity and cycle performance of bio-based hard carbon sodium-ion battery anode materials, increases the graphite interlayer spacing, provides more sodium-ion storage sites, and improves rate performance and first coulombic efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993028A_ABST
    Figure CN118993028A_ABST
Patent Text Reader

Abstract

The invention discloses a biological matrix hard carbon sodium ion battery negative electrode material and a preparation method thereof, and the method comprises the following steps: (1) pre-carbonization: crushing and sieving coconut shells, and then carrying out low-temperature carbonization treatment to prepare first pre-carbonized powder; (2) soaking with sulfuric acid: crushing and sieving the first pre-carbonized powder again, soaking with sulfuric acid, washing, and drying to obtain second pre-carbonized powder; and (3) a high-temperature heat treatment and sulfur doping process: putting the second pre-carbonized powder and elemental sulfur powder into a vacuum tube furnace, and performing high-temperature carbonization and sulfur doping in an inert gas atmosphere to prepare a sulfur-doped hard carbon negative electrode material crude product. The coconut shell with low impurity content and high strength is selected as the negative electrode precursor, and the pore structure, the surface oxygen-containing functional group and the graphite microcrystalline structure of the biomass hard carbon are regulated and controlled by regulating and controlling the high-temperature heat treatment temperature and the sulfur doping process, so that the reversible capacity, the first coulombic efficiency, the cycle performance and the like of the sodium ion battery can be remarkably improved; the service life is prolonged.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of negative electrode materials for sodium ion batteries, and in particular to a negative electrode material for a biomatrix hard carbon sodium ion battery and a preparation method thereof. Background Art

[0002] Sodium-ion batteries have the advantages of large sodium storage capacity, easy large-scale production and application, and are considered to be potential candidate materials in the field of energy storage. However, the lack of suitable negative electrode materials has hindered the rapid development of sodium-ion batteries to a certain extent. As in the case of lithium-ion batteries, the selection of negative electrode materials is more demanding than that of positive electrode materials because the selection range of positive electrode materials is very wide. The ideal negative electrode material for sodium-ion batteries should meet the characteristics of low reaction potential, large reversible capacity, stable cycle performance, high conductivity, stable structure, high safety performance, low price, and wide range of raw materials. Although a large number of negative electrode materials such as metal compounds, alloy compounds and organic compounds have been reported as sodium-ion batteries, most of them face problems such as high cost and environmental pollution. In contrast, carbonaceous materials have the advantages of high capacity, abundant resources, non-toxicity, low cost and environmental friendliness, which are more attractive for industrial production applications. The molecular configuration of the precursor affects the graphite microcrystalline structure of hard carbon materials, which is characterized by the presence of many randomly oriented graphite regions and disordered structural carbon with residual heteroatoms on the surface. The mixture of graphite microcrystalline structure and disordered structure of hard carbon provides a large number of intrinsic defects, nanopores and large interlayer spacing, thus providing more sodium ion diffusion paths and sodium ion storage sites. Therefore, it is urgent to develop a biomass-based hard carbon sodium ion battery anode material with high specific capacity and excellent cycle performance to meet the current demand for sodium ion batteries in the new energy field. Summary of the invention

[0003] In order to solve the above-mentioned problem that the existing sodium ion batteries lack suitable negative electrode materials, and most of the existing negative electrode materials for sodium ion batteries face the problems of high cost and environmental pollution, the present invention provides a bio-matrix hard carbon sodium ion battery negative electrode material and a preparation method thereof, and selects coconut shell with low impurity content and high inherent strength as the precursor of the negative electrode material for the sodium ion battery. By adjusting the high-temperature heat treatment temperature and the sulfur doping process, the pore structure, surface oxygen-containing functional groups and graphite microcrystalline structure of the biomass hard carbon are regulated to achieve high reversible capacity and high rate performance of the negative electrode material for the sodium ion battery.

[0004] To achieve the above object, the present invention provides the following technical solutions: A method for preparing a biomatrix hard carbon sodium ion battery negative electrode material, characterized in that it comprises the following steps: (1) Pre-carbonization: First, the raw coconut shell is crushed and sieved, and then the sieved coconut shell raw material is placed in a carbonization furnace for low-temperature carbonization treatment for 2 to 4 hours, and then taken out after cooling to room temperature to obtain the first pre-carbonized powder; (2) Soaking in sulfuric acid: The first pre-carbonized powder obtained in step 1 is crushed again and sieved, soaked in sulfuric acid for 0.5 to 1 hour, washed with ultrapure water, and then transferred to a vacuum drying oven for drying for 7 to 8 hours to obtain a second pre-carbonized powder; (3) High-temperature heat treatment and sulfur doping process: The second pre-carbonized powder and elemental sulfur powder obtained in step 2 are placed in a vacuum tube furnace. The air in the furnace is first extracted by a vacuum pump, and then an inert gas is continuously introduced into the furnace to prevent air from entering the furnace. The second pre-carbonized powder is always placed in an inert gas atmosphere for high-temperature carbonization and sulfur doping. After the high-temperature heat treatment is completed, the powder is cooled to room temperature and taken out to obtain a crude sulfur-doped hard carbon negative electrode material; (4) Washing and drying: The crude sulfur-doped hard carbon negative electrode material obtained in step 3 is washed with ultrapure water and then transferred to a vacuum drying oven for 7 to 8 hours. After drying, it is sieved through a 350 to 400 mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material; (5) Preparing negative electrode slurry: The finished sulfur-doped hard carbon negative electrode material prepared in step 4 is weighed and mixed with a conductive agent and a binder in a ratio of 7-8:1-1.5:1-1.5, and a solvent N-methylpyrrolidone (NMP) is added dropwise to mix and slurry to prepare a negative electrode slurry for a sodium ion battery.

[0005] Preferably, the coconut shell raw material after crushing and screening in step (1) needs to be washed and dried with ultrapure water before low-temperature carbonization.

[0006] Preferably, the low-temperature carbonization temperature of the raw coconut shell in step (1) is 400-800°C, and the temperature rise rate is 5-10°C / min.

[0007] Preferably, the powder is pulverized through a 80-100 mesh sieve in step (1); and further pulverized through a 100-120 mesh sieve in step (2).

[0008] Preferably, the concentration of sulfuric acid in step (2) is 0.1 to 1 mol / L.

[0009] Preferably, the conductivity of the filtrate after washing in step (2) is 1 to 20 μS / cm.

[0010] Preferably, in step (3), the mass ratio of the second pre-carbonized powder to the elemental sulfur powder is 1:2-3.

[0011] Preferably, in step (3), the elemental sulfur powder is placed at the front end position along the direction of the inert gas flow.

[0012] Preferably, in step (3), the high temperature heat treatment temperature is 1300-1500° C., the heating rate is 5-10° C. / min, and the holding time is 1-5 h.

[0013] The present invention also provides a biomatrix hard carbon sodium ion battery negative electrode material, characterized in that: the biomatrix hard carbon sodium ion battery negative electrode material is prepared by the above-mentioned preparation method.

[0014] Compared with the prior art, the beneficial effects of the present invention are as follows: the present invention pre-carbonizes the raw materials, washes them with sulfuric acid, and then performs high-temperature heat treatment, and simultaneously dopes sulfur in the process, finally obtaining a sulfur-doped hard carbon negative electrode material, and finally assembling the battery to test the electrochemical performance. The results show that the sulfur-doped hard carbon negative electrode material has a larger graphite interlayer spacing and more sodium storage active sites, and not only has a larger reversible sodium storage capacity, but also has significant improvements in rate and cycle performance.

[0015] 1. The present invention selects coconut shell with low impurity content and high self-strength as the precursor of the negative electrode material of the sodium ion battery. Through the sulfur doping process, the microstructures such as pores, defects and interlayer spacing have changed. Sulfur doping can not only provide more sodium storage active sites, but also increase the interlayer spacing of the graphite microcrystalline structure, thereby improving the storage capacity of sodium ions. 2. The present invention regulates the graphite microcrystal structure, including the pore structure of biomass hard carbon, the interlayer spacing of graphite microcrystals and the concentration of surface oxygen-containing functional groups, by adjusting the high-temperature heat treatment temperature and the sulfur doping process, which can significantly improve its reversible capacity, first coulombic efficiency and cycle performance, and extend the service life of sodium ion batteries. BRIEF DESCRIPTION OF THE DRAWINGS

[0016] Figure 1 This is a SEM image of the coconut shell-based biomass hard carbon negative electrode material prepared in Example 1 of the present invention; Figure 2 This is a HRTEM image of the coconut shell-based biomass hard carbon negative electrode material prepared in Example 1 of the present invention; Figure 3 This is a comparison chart of the rate performance of coconut shell-based biomass hard carbon prepared in Example 1 of the present invention and Comparative Example 1; Figure 4 This is a comparison chart of the cycle performance of coconut shell-based biomass hard carbon prepared in Example 1 of the present invention and Comparative Example 1; Figure 5 This is a constant current charge-discharge curve of the first cycle of coconut shell-based biomass hard carbon prepared in Example 1 of the present invention; Figure 6 This is a constant current charge and discharge curve of the first cycle of coconut shell-based biomass hard carbon prepared in Comparative Example 2 of the present invention. DETAILED DESCRIPTION

[0017] In order to facilitate the understanding of the present invention, the present invention will be described more comprehensively and meticulously below in conjunction with the accompanying drawings and preferred embodiments of the specification, but the protection scope of the present invention is not limited to the following specific embodiments.

[0018] Unless otherwise defined, all the professional terms used below have the same meaning as those generally understood by those skilled in the art. The professional terms used herein are only for the purpose of describing specific embodiments and are not intended to limit the scope of protection of the present invention.

[0019] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in the present invention can be purchased from the market or prepared by existing methods. Example

[0020] A method for preparing a biomatrix hard carbon sodium ion battery negative electrode material comprises the following steps: (1) Pre-carbonization: First, the raw coconut shell is crushed by a crusher, passed through an 80-mesh sieve, washed with ultrapure water, and transferred to a vacuum drying oven for drying. The dried coconut shell raw material is then placed in a carbonization furnace for low-temperature carbonization treatment. The carbonization temperature is 400°C, the heating rate is 5°C / min, and the insulation time is 2h. After cooling to room temperature, it is taken out to obtain a first pre-carbonized powder; (2) Soaking in sulfuric acid: The first pre-carbonized powder obtained in step 1 was crushed again and passed through a 120-mesh sieve, and then soaked in 0.5 mol / L sulfuric acid for 1 hour. After washing with ultrapure water, the powder was transferred to a vacuum drying oven and dried for 7 to 8 hours to obtain a second pre-carbonized powder. The conductivity of the filtrate after washing was 19 μS / cm. (3) High-temperature heat treatment and sulfur doping process: The second pre-carbonized powder obtained in step 2 and the elemental sulfur powder are placed in a vacuum tube furnace in a mass ratio of 1:2, and the elemental sulfur powder is placed at the front end along the direction of the argon gas flow. The air in the furnace is first extracted by a vacuum pump, and then argon gas is continuously introduced into the furnace to prevent air from entering the furnace. The second pre-carbonized powder is always placed in an argon atmosphere for high-temperature carbonization and sulfur doping. The final carbonization temperature is 1400°C, the heating rate is 5°C / min, and the insulation time is 2h. After the high-temperature heat treatment is completed, it is cooled to room temperature and taken out to obtain a crude sulfur-doped hard carbon negative electrode material; (4) Washing and drying: The crude sulfur-doped hard carbon negative electrode material obtained in step 3 is washed with ultrapure water and then transferred to a vacuum drying oven for drying for 8 hours. After drying, the crude sulfur-doped hard carbon negative electrode material is sieved through a 350-mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material. (5) Preparation of negative electrode slurry: The finished sulfur-doped hard carbon negative electrode material obtained in step 4 is weighed and mixed with a conductive agent and a binder in a ratio of 8:1:1, and a solvent N-methylpyrrolidone (NMP) is added dropwise to mix and slurry for 12 hours to obtain a negative electrode slurry for a sodium ion battery.

[0021] Figure 1 , 2 They are respectively the SEM image and HRTEM image of the coconut shell-based biomass hard carbon negative electrode material during the preparation process of Example 1. Example

[0022] A method for preparing a biomatrix hard carbon sodium ion battery negative electrode material comprises the following steps: (1) Pre-carbonization: First, the raw coconut shell is crushed with a crusher, then washed with ultrapure water and passed through an 80-mesh sieve, and then the sieved coconut shell raw material is placed in a carbonization furnace for low-temperature carbonization treatment. The carbonization temperature is 500°C, the heating rate is 7°C / min, and the insulation time is 2h. After cooling to room temperature, it is taken out to obtain the first pre-carbonized powder; (2) Soaking in sulfuric acid: The first pre-carbonized powder obtained in step 1 was crushed again and passed through a 120-mesh sieve, soaked in 0.5 mol / L sulfuric acid for 1 h, washed with ultrapure water, and then transferred to a vacuum drying oven for drying for 8 h to obtain a second pre-carbonized powder; the conductivity of the filtrate after washing was 16 μS / cm; (3) High-temperature heat treatment and sulfur doping process: The second pre-carbonized powder obtained in step 2 and the elemental sulfur powder are placed in a vacuum tube furnace in a mass ratio of 1:3, and the elemental sulfur powder is placed at the front end along the direction of the argon gas flow. The air in the furnace is first extracted by a vacuum pump, and then argon gas is continuously introduced into the furnace to prevent air from entering the furnace. The second pre-carbonized powder is always in an argon atmosphere for high-temperature carbonization and sulfur doping. The final carbonization temperature is 1400°C, the heating rate is 5°C / min, and the insulation time is 3h. After the high-temperature heat treatment is completed, it is cooled to room temperature and taken out to obtain a crude sulfur-doped hard carbon negative electrode material; (4) Washing and drying: The crude sulfur-doped hard carbon negative electrode material obtained in step 3 is washed with ultrapure water and then transferred to a vacuum drying oven for drying for 8 hours. After drying, the crude sulfur-doped hard carbon negative electrode material is sieved through a 350-mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material. (5) Preparation of negative electrode slurry: The finished sulfur-doped hard carbon negative electrode material obtained in step 4 was weighed and mixed with a conductive agent and a binder in a ratio of 8:1:1, and solvent N-methylpyrrolidone (NMP) was added dropwise to mix and slurry for 16 hours to obtain a negative electrode slurry for a sodium ion battery. Example

[0023] A method for preparing a biomatrix hard carbon sodium ion battery negative electrode material comprises the following steps: (1) Pre-carbonization: First, the raw coconut shell is crushed by a crusher, then washed with ultrapure water and passed through an 80-mesh sieve, and then the sieved coconut shell raw material is placed in a carbonization furnace for low-temperature carbonization treatment. The carbonization temperature is 600°C, the heating rate is 10°C / min, and the insulation time is 2h. After cooling to room temperature, it is taken out to obtain the first pre-carbonized powder; (2) Soaking in sulfuric acid: The first pre-carbonized powder obtained in step 1 was crushed again and passed through a 120-mesh sieve, and then soaked in 0.5 mol / L sulfuric acid for 0.8 h. After washing with ultrapure water, the powder was transferred to a vacuum drying oven and dried for 8 h to obtain a second pre-carbonized powder. The conductivity of the filtrate after washing was 18 μS / cm. (3) High-temperature heat treatment and sulfur doping process: The second pre-carbonized powder obtained in step 2 and the elemental sulfur powder are placed in a vacuum tube furnace in a mass ratio of 1:2, and the elemental sulfur powder is placed at the front end along the direction of the argon gas flow. The air in the furnace is first extracted by a vacuum pump, and then argon gas is continuously introduced into the furnace to prevent air from entering the furnace. The second pre-carbonized powder is always in an argon atmosphere for high-temperature carbonization and sulfur doping. The final carbonization temperature is 1400°C, the heating rate is 8°C / min, and the insulation time is 2h. After the high-temperature heat treatment is completed, it is cooled to room temperature and taken out to obtain a crude sulfur-doped hard carbon negative electrode material; (4) Washing and drying: The crude sulfur-doped hard carbon negative electrode material obtained in step 3 is washed with ultrapure water and then transferred to a vacuum drying oven for drying for 8 hours. After drying, the crude sulfur-doped hard carbon negative electrode material is sieved through a 350-mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material. (5) Preparation of negative electrode slurry: The finished sulfur-doped hard carbon negative electrode material obtained in step 4 was weighed and mixed with a conductive agent and a binder in a ratio of 8:1:1, and solvent N-methylpyrrolidone (NMP) was added dropwise to mix and slurry for 10 hours to obtain a negative electrode slurry for a sodium ion battery. Example

[0024] The process is basically the same as Example 1, except that the final carbonization temperature in step (3) is 1300°C. Example

[0025] The method is basically the same as Example 1, except that in step (5), the finished sulfur-doped hard carbon negative electrode material is mixed with the conductive agent and the binder in a ratio of 7:1.5:1.5 for 12 hours. Example

[0026] The method is basically the same as Example 1, except that: in step (4), after drying, the product is sieved through a 400-mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material.

[0027] Comparative Example 1: The step (3) in Example 1 is changed to placing the second pre-carbonized powder (excluding the elemental sulfur powder) into a vacuum tube furnace for high-temperature heat treatment, i.e., no sulfur doping process is performed. Other conditions are the same as in Example 1.

[0028] Comparative Example 2: The process is basically the same as Example 1, except that the final temperature of high temperature carbonization in step (3) is 1200°C.

[0029] Comparative Example 3: The method is basically the same as Example 1, except that the final temperature of high temperature carbonization in step (3) is 1600°C.

[0030] Performance Testing: The sodium ion battery negative electrode slurry prepared in Examples 1 to 6 and Comparative Examples 1 to 3 was coated and dried, and then punched into 16 mm electrode sheets, and button batteries were formed with sodium metal sheets, ester electrolytes, diaphragms and other materials, and their electrochemical properties were tested. The measurement results are shown in Tables 1 and Figures 3 to 6 .

[0031] Table 1

[0032] Note: The reversible capacity in Table 1 is at a current density of 0.02 A g −1 The cycle performance was measured at a current density of 2A·g −1 Measured below.

[0033] As can be seen from Table 1, the reversible capacity, first coulombic efficiency and capacity retention rate after 200 cycles of the biomatrix hard carbon sodium ion battery negative electrode materials prepared in Examples 1 to 6 of the present invention are greater than those in Comparative Example 1. Through the sulfur doping process, the microstructures such as pores, defects and interlayer spacing have changed. Sulfur doping can not only provide more sodium storage active sites, but also increase the interlayer spacing of the graphite microcrystalline structure, effectively improve its reversible capacity, and also optimize its rate performance and first coulombic efficiency. It can also be seen from Table 1 that the reversible capacity, first coulombic efficiency and capacity retention rate after 200 cycles of the biomatrix hard carbon sodium ion battery negative electrode material prepared by Examples 1 to 6 of the present invention are greater than those of Comparative Examples 2 and 3, and the process of high-temperature heat treatment and sulfur doping of the pre-carbonized material is crucial. The high-temperature heat treatment temperature itself plays a very important role in the regulation of the microstructure of biomass hard carbon. With the increase of the high-temperature heat treatment temperature, the surface defect concentration of coconut shell-based hard carbon drops sharply, such as the reduction of the concentration of surface oxygen-containing functional groups, the collapse of the pore structure, etc. By adjusting the high-temperature heat treatment temperature, the graphite interlayer spacing is reduced to a suitable size, which can not only meet the embedding and extraction process of sodium ions, but also eliminate most of the adsorption process of pseudo-graphite structures, significantly improving its first coulombic efficiency; however, after the doping of sulfur element, sulfur is embedded in the graphite interlayer or reacts with the carbon layer to form sulfur-containing functional groups and sulfur-sulfur bonds, which provides more active sites for the storage of sodium ions and can significantly synergistically improve its reversible capacity. Even though the doping of sulfur elements will introduce defects and a higher specific surface area, resulting in the generation of more solid electrolyte interface films, the increase in the interlayer spacing will significantly increase the proportion of reversible capacity, so the doping of sulfur elements can also improve the first coulombic efficiency.

[0034] Through the above process design, coconut shell-based hard carbon negative electrode materials with high reversible capacity and excellent rate cycling performance can be obtained, which provides new insights into the design of high energy density sodium ion battery negative electrode materials.

[0035] The above are only preferred embodiments of the present invention. It should be pointed out that, for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.

Claims

1. A method for preparing a negative electrode material for a biomatrix hard carbon sodium ion battery, characterized in that: The following steps are involved: (1) Pre-carbonization: First, the raw coconut shell is crushed and sieved, and then the sieved coconut shell raw material is placed in a carbonization furnace for low-temperature carbonization treatment for 2 to 4 hours, and then taken out after cooling to room temperature to obtain the first pre-carbonized powder; (2) Soaking in sulfuric acid: The first pre-carbonized powder obtained in step 1 is crushed again and sieved, soaked in sulfuric acid for 0.5 to 1 hour, washed with ultrapure water, and then transferred to a vacuum drying oven for drying for 7 to 8 hours to obtain a second pre-carbonized powder; (3) High-temperature heat treatment and sulfur doping process: The second pre-carbonized powder and elemental sulfur powder obtained in step 2 are placed in a vacuum tube furnace. The air in the furnace is first extracted by a vacuum pump, and then an inert gas is continuously introduced into the furnace to prevent air from entering the furnace. The second pre-carbonized powder is always placed in an inert gas atmosphere for high-temperature carbonization and sulfur doping. After the high-temperature heat treatment is completed, the powder is cooled to room temperature and taken out to obtain a crude sulfur-doped hard carbon negative electrode material; (4) Washing and drying: The crude sulfur-doped hard carbon negative electrode material obtained in step 3 is washed with ultrapure water and then transferred to a vacuum drying oven for 7 to 8 hours. After drying, it is sieved through a 350 to 400 mesh sieve to obtain a finished sulfur-doped hard carbon negative electrode material; (5) Preparing negative electrode slurry: The finished sulfur-doped hard carbon negative electrode material prepared in step 4 is weighed and mixed with a conductive agent and a binder in a ratio of 7-8:1-1.5:1-1.5, and a solvent N-methylpyrrolidone (NMP) is added dropwise to mix and slurry to prepare a negative electrode slurry for a sodium ion battery.

2. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: The coconut shell raw material after crushing and screening in the step (1) needs to be washed and dried with ultrapure water before low-temperature carbonization.

3. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: In the step (1), the low-temperature carbonization temperature of the raw coconut shell is 400-800°C, and the temperature rise rate is 5-10°C / min.

4. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: In the step (1), the powder is crushed through a 80-100 mesh sieve; and in the step (2), the powder is crushed through a 100-120 mesh sieve.

5. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: The concentration of sulfuric acid in step (2) is 0.1 to 1 mol / L.

6. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: The conductivity of the filtrate after washing in the step (2) is 1 to 20 μS / cm.

7. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: In the step (3), the mass ratio of the second pre-carbonized powder to the elemental sulfur powder is 1:2-3.

8. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: In the step (3), the elemental sulfur powder is placed at the front end along the direction of the inert gas flow.

9. The method for preparing a biomatrix hard carbon sodium ion battery negative electrode material according to claim 1, characterized in that: In the step (3), the high temperature heat treatment temperature is 1300-1500° C., the heating rate is 5-10° C. / min, and the holding time is 1-5 h.

10. A biomatrix hard carbon sodium ion battery negative electrode material, characterized in that: The biomatrix hard carbon sodium ion battery negative electrode material is prepared by the preparation method according to any one of claims 1 to 8.