Nitrogen-doped porous carbon sphere material, preparation method and application thereof, and lithium ion battery negative electrode material
The corn core hemicellulose was extracted through ultrasonic assisted alkali method and modified by N2 plasma technology to prepare nitrogen-doped porous carbon ball material, which solved the problems of complexity and pollution in traditional processes and achieved a high ratio of the negative electrode material of lithium-ion batteries Capacity and low pollution production.
Patent Information
- Application Number
- CN202411316011.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-20
- Publication Date
- 2024-11-22
AI Technical Summary
The preparation process of traditional biomass porous carbon sphere materials is complex and polluted the environment, making it difficult to achieve green and environmentally friendly utilization of corn cob hemicellulose, affecting the large-scale industrial production of biomass carbon materials.
Ultrasonic assisted alkali method to extract corncob hemicellulose, prepare biomass-based carbon sphere materials through hydrothermal carbonization, and use N2 plasma technology to perform surface modification, increase specific surface area and nitrogen content, and form nitrogen-doped porous carbon Ball material.
It realizes the preparation of nitrogen-doped porous carbon ball materials with low cost, low pollution and easy operation, and increases the specific capacity and surface functionality of the negative electrode material of lithium-ion battery, which is suitable for large-scale production.
Smart Images

Figure CN118993032A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of porous carbon materials, and in particular relates to a nitrogen-doped porous carbon ball material, a preparation method and application thereof, and a negative electrode material for a lithium-ion battery. Background Art
[0002] Biomass carbon materials have attracted widespread attention due to their abundant reserves and green environmental protection. There are many types of biomass raw materials, among which corn cobs are a by-product of corn processing. The annual output is huge, which leads to serious environmental pollution caused by littering and open-air burning of corn cobs. How to effectively and harmlessly utilize and treat corn cobs has always been the focus of research. The main components of corn cobs are cellulose, hemicellulose and lignin. The separated cellulose is a polymer compound composed of glucose, which can be used to prepare alcohol and other chemical products; while hemicellulose is mostly discarded as waste, resulting in a waste of resources. In fact, hemicellulose, as one of the abundant natural polymer renewable energy sources on the earth, has unique structural characteristics and physiological activity. After modification, it can be used in food, medicine, tissue engineering and other fields. It is a high value-added material to replace traditional petrochemical products.
[0003] At present, biomass carbon materials have broad application prospects in many fields such as batteries and supercapacitors. Studies have found that the microstructure and specific surface area of biomass carbon will affect the electrochemical properties of biomass carbon materials. Therefore, designing and preparing high-performance biomass carbon materials with porous structures is the key to energy shortage and environmental protection. Biomass porous carbon has a variety of structural characteristics, among which porous carbon spheres combine the dual advantages of spherical structure and porous structure, and have better structural stability and surface chemical properties. Therefore, porous carbon spheres have become a key raw material in the field of electrode material research.
[0004] Traditional biomass porous carbon spheres are prepared by chemical activation and physical activation, which are complex and environmentally friendly. How to use hemicellulose in corn cobs to prepare porous carbon spheres in a greener and more environmentally friendly way is still an urgent problem to be solved in the process of large-scale industrial production of biomass carbon materials. Summary of the invention
[0005] In order to solve the problems of complex operation and environmental pollution in the existing activation process for preparing porous carbon spheres, the present invention provides a nitrogen-doped porous carbon sphere material, a preparation method and application thereof, and a lithium-ion battery negative electrode material.
[0006] The technical solution of the present invention:
[0007] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0008] Step 1: Prepare hemicellulose pretreatment solution:
[0009] The corn cob is dried and crushed, and the obtained powder sample is dispersed in a sodium hydroxide solution and subjected to ultrasonic treatment to obtain a hemicellulose pretreatment solution;
[0010] Step 2: Preparation of biomass-based carbon ball materials:
[0011] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath for heating reaction, cooled to room temperature after the reaction is completed, filtered and collected by suction, an acetic acid-ethanol mixed solution is added to the obtained filtrate, and a precipitate is precipitated by standing, the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water, concentrated sulfuric acid is added to adjust the pH, and then a hydrothermal reaction is carried out, and after the reaction is completed, the precipitate is filtered and collected, and washed and dried to obtain a biomass-based carbon ball material;
[0012] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0013] The biomass-based carbon sphere material obtained in step 2 is modified under plasma and nitrogen atmosphere to obtain a nitrogen-doped porous carbon sphere material.
[0014] Furthermore, in step 1, the particle size of the powder sample is 500-1000 μm, the concentration of the sodium hydroxide solution is 50-100 g / L, and the solid-liquid ratio of the powder sample to the sodium hydroxide solution is 1 g:20-30 mL.
[0015] Furthermore, the temperature of the ultrasonic treatment in step 1 is 40-60° C., and the ultrasonic time is 0.5-2 h.
[0016] Furthermore, the heating reaction in step 2 is carried out at a temperature of 70 to 90° C. for 1 to 3 hours under water bath conditions; and the volume ratio of acetic acid to ethanol in the acetic acid-ethanol mixed solution is 1:9.
[0017] Furthermore, the solid-liquid ratio of the precipitate to water in step 2 is 1 g:5-25 mL, and the addition of concentrated sulfuric acid to adjust the pH is to adjust the pH to 1-3.
[0018] Furthermore, the temperature of the hydrothermal reaction in step 2 is 180° C., and the reaction time is 4 to 20 hours.
[0019] Furthermore, in step three, the power of the plasma is 30 W, and the modification time is 20 min.
[0020] A nitrogen-doped porous carbon ball material prepared by the preparation method provided by the invention has a nitrogen doping amount of 1-5% and an average particle size of the carbon ball of 3-5 μm.
[0021] The invention discloses an application of the nitrogen-doped porous carbon sphere material prepared by the invention in the field of negative electrode materials for lithium-ion batteries.
[0022] A lithium ion battery negative electrode material comprises the nitrogen-doped porous carbon ball material prepared by the invention.
[0023] Beneficial effects of the present invention:
[0024] The present invention uses biomass corn cobs as raw materials, extracts hemicellulose from corn cobs by ultrasound-assisted alkaline method as a carbon material precursor, converts hemicellulose into biomass-based carbon ball materials by hydrothermal carbonization under the condition of adding an acidic catalyst, and finally uses N2 plasma technology to perform surface modification on the carbon balls. After the modification, the specific surface area of the carbon balls is increased, the nitrogen content is increased, and the specific capacity is significantly increased when the carbon balls are used as negative electrode materials for lithium-ion batteries, which can reach 232.1 mAh g -1 .
[0025] The present invention uses biomass waste corn cobs as carbon sources, which have the advantages of low cost, high reserves and renewability, and solves the problems of environmental pollution caused by the treatment of corn cobs; N2 plasma technology is used as a modification treatment technology, and nitrogen atoms are introduced into the carbon ball material while etching the surface of the material to improve the surface function of the material and increase the specific surface area of the material. The method is easy to operate, highly efficient and pollution-free, and can be carried out at room temperature, which is conducive to the large-scale industrial production of nitrogen-doped porous carbon ball materials. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] Figure 1 This is a SEM image of the biomass-based carbon sphere material prepared in Example 1;
[0027] Figure 2 This is a SEM image of the nitrogen-doped porous carbon sphere material prepared in Example 1;
[0028] Figure 3 This is a nitrogen adsorption-desorption curve diagram of the nitrogen-doped porous carbon sphere material prepared in Example 1;
[0029] Figure 4 This is the elemental analysis XPS graph of the nitrogen-doped porous carbon sphere material prepared in Example 1;
[0030] Figure 5 The negative electrode material of the lithium ion battery prepared in Example 14 is 0.1Ag -1 Cycle curve diagram of
[0031] Figure 6 This is a rate cycle diagram of the lithium-ion battery negative electrode material prepared in Example 1 at different current densities. DETAILED DESCRIPTION
[0032] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0033] Example 1
[0034] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0035] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0036] Step 1: Prepare hemicellulose pretreatment solution:
[0037] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0038] Step 2: Preparation of biomass-based carbon ball materials:
[0039] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0040] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0041] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain a nitrogen-doped porous carbon sphere material. The nitrogen doping amount was 3.02%, and the obtained carbon sphere yield was 26.14%.
[0042] Figure 1 This is a SEM image of the biomass-based carbon sphere material prepared in Example 1, which shows that the carbon spheres are uniform in shape and smooth in surface, with an average particle size of about 3-5 μm.
[0043] Figure 2This is a SEM image of the nitrogen-doped porous carbon sphere material prepared in Example 1. The image shows that the carbon sphere remains spherical after modification, and many microporous structures are generated on the surface, increasing the roughness of the material surface. This is because plasma bombardment of the material surface will cause a series of etching effects, forming defects or pores on the surface of the material.
[0044] Figure 3 The nitrogen adsorption-desorption curve of the nitrogen-doped porous carbon sphere material prepared in Example 1 shows that the nitrogen-doped porous carbon sphere exhibits a Langmuir III isotherm, indicating that the pore structure of the modified sample is mesoporous and the specific surface area is 37.6488 m 2 / g. The adsorption amount of sample ACS increased significantly at higher pressure, indicating that there are more pores in ACS.
[0045] Figure 4 This is the elemental analysis XPS graph of the nitrogen-doped porous carbon sphere material prepared in Example 1, which shows that the nitrogen element is successfully doped into the carbon sphere material, and compared with the unmodified carbon sphere, the N atom content of the nitrogen-doped porous carbon sphere is significantly increased, which indicates that under the action of nitrogen plasma, N2 is ionized to fix N on the surface of the carbon sphere, thereby increasing the nitrogen-containing functional groups on its surface.
[0046] Example 2
[0047] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0048] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0049] Step 1: Prepare hemicellulose pretreatment solution:
[0050] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0051] Step 2: Preparation of biomass-based carbon ball materials:
[0052] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:5mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0053] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0054] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 18.83%.
[0055] Example 3
[0056] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0057] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0058] Step 1: Prepare hemicellulose pretreatment solution:
[0059] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0060] Step 2: Preparation of biomass-based carbon ball materials:
[0061] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:15mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0062] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0063] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 14.77%.
[0064] Example 4
[0065] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0066] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0067] Step 1: Prepare hemicellulose pretreatment solution:
[0068] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0069] Step 2: Preparation of biomass-based carbon ball materials:
[0070] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:20mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0071] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0072] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 14.84%.
[0073] Example 5
[0074] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0075] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0076] Step 1: Prepare hemicellulose pretreatment solution:
[0077] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0078] Step 2: Preparation of biomass-based carbon ball materials:
[0079] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:25mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0080] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0081] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 13.58%.
[0082] Example 6
[0083] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0084] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0085] Step 1: Prepare hemicellulose pretreatment solution:
[0086] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0087] Step 2: Preparation of biomass-based carbon ball materials:
[0088] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for reaction for 3 hours. After the reaction is completed, it is cooled to room temperature, and the filtrate is collected by suction. An acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is allowed to stand to precipitate. The precipitate is collected by suction, washed and dried, and then dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1, and then a hydrothermal reaction is carried out. After reacting at 180°C for 12 hours, the precipitate is collected by filtration and washed and dried to obtain a biomass-based carbon ball material;
[0089] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0090] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 26.04%.
[0091] Example 7
[0092] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0093] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0094] Step 1: Prepare hemicellulose pretreatment solution:
[0095] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0096] Step 2: Preparation of biomass-based carbon ball materials:
[0097] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 2, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0098] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0099] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 21.27%.
[0100] Example 8
[0101] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0102] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0103] Step 1: Prepare hemicellulose pretreatment solution:
[0104] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0105] Step 2: Preparation of biomass-based carbon ball materials:
[0106] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for reaction for 3 hours. After the reaction is completed, it is cooled to room temperature, and the filtrate is collected by suction. An acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is allowed to stand to precipitate. The precipitate is collected by suction, washed and dried, and then dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 2.5, and then a hydrothermal reaction is carried out. After reacting at 180°C for 12 hours, the precipitate is collected by filtration and washed and dried to obtain a biomass-based carbon ball material;
[0107] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0108] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 13.47%.
[0109] Example 9
[0110] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0111] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0112] Step 1: Prepare hemicellulose pretreatment solution:
[0113] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0114] Step 2: Preparation of biomass-based carbon ball materials:
[0115] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 3, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0116] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0117] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 11.96%.
[0118] Example 10
[0119] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0120] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0121] Step 1: Prepare hemicellulose pretreatment solution:
[0122] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0123] Step 2: Preparation of biomass-based carbon ball materials:
[0124] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0125] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0126] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 2.1%.
[0127] Embodiment 11
[0128] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0129] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0130] Step 1: Prepare hemicellulose pretreatment solution:
[0131] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0132] Step 2: Preparation of biomass-based carbon ball materials:
[0133] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for reaction for 3 hours. After the reaction is completed, it is cooled to room temperature, and the filtrate is collected by suction. An acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is allowed to stand to precipitate. The precipitate is collected by suction, washed and dried, and then dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out. After reacting at 180°C for 8 hours, the precipitate is collected by filtration and washed and dried to obtain a biomass-based carbon ball material;
[0134] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0135] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 10.46%.
[0136] Example 12
[0137] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0138] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0139] Step 1: Prepare hemicellulose pretreatment solution:
[0140] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0141] Step 2: Preparation of biomass-based carbon ball materials:
[0142] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0143] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0144] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 26.11%.
[0145] Embodiment 13
[0146] This embodiment provides a nitrogen-doped porous carbon sphere material and a preparation method thereof.
[0147] A method for preparing a nitrogen-doped porous carbon sphere material comprises the following steps:
[0148] Step 1: Prepare hemicellulose pretreatment solution:
[0149] The corn cob was dried and crushed to obtain a powder sample with a particle size of 500 μm, and the obtained powder sample was dispersed in 80 g / L sodium hydroxide solution at a solid-liquid ratio of 1 g:25 mL, and ultrasonically treated at 50° C. for 0.5 h to obtain a hemicellulose pretreatment solution;
[0150] Step 2: Preparation of biomass-based carbon ball materials:
[0151] The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath at 80°C for 3 hours, cooled to room temperature after the reaction is completed, and the filtrate is collected by suction, and an acetic acid-ethanol mixed solution with a volume ratio of acetic acid to ethanol of 1:9 is added to the obtained filtrate, and the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water at a solid-liquid ratio of 1g:10mL, concentrated sulfuric acid is added to adjust the pH to 1.5, and then a hydrothermal reaction is carried out, and the precipitate is collected by filtering and washed and dried to obtain a biomass-based carbon ball material;
[0152] Step 3: Preparation of nitrogen-doped porous carbon sphere material:
[0153] The biomass-based carbon sphere material obtained in step 2 was modified under 30W plasma and nitrogen atmosphere for 20 minutes to obtain nitrogen-doped porous carbon sphere material, and the yield of the obtained carbon spheres was 26.24%.
[0154] Embodiment 14
[0155] This embodiment provides a lithium ion battery negative electrode material comprising the nitrogen-doped porous carbon material prepared in Example 1.
[0156] In this embodiment, the negative electrode material of the lithium ion battery is prepared by mixing the nitrogen-doped porous carbon ball material prepared in Example 1, acetylene black and polyvinylidene fluoride in a mass ratio of 8:1:1.
[0157] Figure 5 The negative electrode material of the lithium ion battery prepared in this embodiment is 0.1Ag -1 The cycle curve after 50 cycles at the current density is 232.1 mAh g -1 . Figure 6 The negative electrode material of the lithium ion battery prepared in this embodiment is 0.1-2Ag. -1 After 10 cycles at each current density, ACS showed a high rate capability at 0.1, 0.2, 0.5, 1, and 2Ag. -1 The reversible capacities under the conditions were 276.5, 252.7, 252.7, 203.9, 138.1 and 67.7 mAh g -1 When the current density increases from 2A -1 Restored to 0.1Ag -1 When the discharge capacity is still up to 275.7 mAh g -1These results demonstrate that the anode material can quickly insert / extract lithium ions, indicating that the nitrogen-doped porous carbon sphere anode material has good rate capability and cycle stability.
Claims
1. A method for preparing nitrogen-doped porous carbon sphere material, characterized in that: The steps include: Step 1: Prepare hemicellulose pretreatment solution: The corn cob is dried and crushed, and the obtained powder sample is dispersed in a sodium hydroxide solution and subjected to ultrasonic treatment to obtain a hemicellulose pretreatment solution; Step 2: Preparation of biomass-based carbon ball materials: The hemicellulose pretreatment liquid obtained in step 1 is placed in a water bath for heating reaction, cooled to room temperature after the reaction is completed, filtered and collected by suction, an acetic acid-ethanol mixed solution is added to the obtained filtrate, and a precipitate is precipitated by standing, the precipitate is collected by suction, washed and dried, and then the precipitate is dispersed in water, concentrated sulfuric acid is added to adjust the pH, and then a hydrothermal reaction is carried out, and after the reaction is completed, the precipitate is filtered and collected, and washed and dried to obtain a biomass-based carbon ball material; Step 3: Preparation of nitrogen-doped porous carbon sphere material: The biomass-based carbon sphere material obtained in step 2 is modified under plasma and nitrogen atmosphere to obtain a nitrogen-doped porous carbon sphere material.
2. The method for preparing a nitrogen-doped porous carbon sphere material according to claim 1, characterized in that: Step 1: The particle size of the powder sample is 500-1000 μm, the concentration of the sodium hydroxide solution is 50-100 g / L, and the solid-liquid ratio of the powder sample to the sodium hydroxide solution is 1 g:20-30 mL.
3. The method for preparing a nitrogen-doped porous carbon sphere material according to claim 1 or 2, characterized in that: The temperature of the ultrasonic treatment in step 1 is 40-60° C., and the ultrasonic time is 0.5-2 h.
4. The method for preparing a nitrogen-doped porous carbon sphere material according to claim 3, characterized in that: The heating reaction in step 2 is carried out under water bath conditions at 70-90° C. for 1-3 hours; the volume ratio of acetic acid to ethanol in the acetic acid-ethanol mixed solution is 1:
9.
5. The method for preparing a nitrogen-doped porous carbon sphere material according to claim 4, characterized in that: In step 2, the solid-liquid ratio of the precipitate to water is 1 g:5-25 mL, and the pH is adjusted to 1-3 by adding concentrated sulfuric acid.
6. The method for preparing a nitrogen-doped porous carbon sphere material according to claim 5, characterized in that: The temperature of the hydrothermal reaction in step 2 is 180° C. and the reaction time is 4 to 20 hours.
7. The method for preparing nitrogen-doped porous carbon sphere material according to claim 6, characterized in that: In step 3, the power of the plasma is 30 W, and the modification time is 20 min.
8. A nitrogen-doped porous carbon sphere material prepared by the preparation method according to any one of claims 1 to 7, characterized in that: The doping amount of nitrogen is 1-5%; the average particle size of the carbon spheres is 3-5 μm.
9. An application of the nitrogen-doped porous carbon sphere material as claimed in claim 8 in the field of negative electrode materials for lithium-ion batteries.
10. A negative electrode material for a lithium ion battery, characterized in that: The method comprises the nitrogen-doped porous carbon sphere material as claimed in claim 8.
Citation Information
Patent Citations
Preparation method and application of hemicellulose based graphitized porous carbon microsphere
CN108751183A
Heteroatom-doped biomass carbon-based electrode material and preparation method and application thereof
CN117602611A
Nitrogen-doped porous carbon as well as preparation method and application thereof
CN118419891A
Preparation method for and use of porous microsphere carbon negative electrode material
WO2023184994A1
Cited By
Corncob-based hard carbon material as well as preparation method and application thereof
CN119750539A
Shell-based nanofiber nitrogen-doped porous carbon material as well as preparation method and application thereof
CN122276687A