Preparation method of FeNiCo-NC micro-nano material and zinc air battery
By using FeNiCo-NC micro/nanomaterials as a catalyst in zinc-air batteries, the problems of high cost and poor stability of existing catalysts have been solved, thus improving the performance and stability of zinc-air batteries.
Patent Information
- Application Number
- CN202410991933.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-23
- Publication Date
- 2024-11-22
AI Technical Summary
Existing commercial platinum-carbon and ruthenium oxide catalysts are expensive and have poor stability, which cannot meet the requirements of zinc-air batteries.
FeNiCo-NC micro/nanomaterials were used as bifunctional catalysts for ORR and OER. Carbon nanotubes were grown in situ on a three-dimensional porous carbon substrate to form a composite structure with excellent hydrophobicity.
It achieves low cost, high performance and good cycle stability, and improves the peak power density and battery performance of zinc-air batteries.
Smart Images

Figure CN118993039A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the field of new energy storage, and specifically relates to the technical field of liquid and quasi-solid secondary zinc-air battery assembly and the technical field of ORR and OER bifunctional catalyst preparation. Background Art
[0002] In recent years, with the further acceleration of electrification, the development of advanced electrochemical energy storage technology and its application scenarios such as grid-scale energy storage, portable electronic devices and electric vehicles have become increasingly important. The past decade has witnessed the great commercial success of energy storage technology, and it has entered the global market in the form of fuel cell electric vehicles and lithium-ion battery electric vehicles. However, the potential danger of lithium-ion batteries limits its application in high-safety fields, such as energy storage power stations, aviation, etc. The high cost of fuel cells has not yet been used on a large scale. Rechargeable zinc-air batteries are low in cost, high in energy density, environmentally friendly, and highly safe, and are considered to be one of the most promising alternatives for the next generation of batteries in energy storage and conversion systems.
[0003] Commercial platinum-carbon and ruthenium oxide (iridium oxide) composite catalysts are currently the most effective ORR / OER bifunctional catalysts. However, metal platinum, ruthenium and iridium are precious metals with extremely high application costs. In addition, the mechanically mixed platinum-carbon and ruthenium oxide cannot be effectively and tightly combined, and have poor stability during use. The performance of the assembled zinc-air battery cannot meet the use requirements. Therefore, it is urgent to develop an ORR and OER bifunctional catalyst that takes into account low cost, good performance and excellent stability. Summary of the invention
[0004] In order to solve the above problems, the present invention provides a preparation method and application of FeNiCo-NC micro-nano material. The quasi-solid-state zinc-air battery with high oxygen reduction and oxygen evolution dual-functional activity, assembled with zinc anode and electrolyte and having a sandwich structure, has excellent peak power density and good cycle stability.
[0005] One of the technical solutions of the present invention is a FeNiCo-NC micro-nano material, in which carbon nanotubes are grown in situ on a three-dimensional porous carbon substrate, and the material has excellent hydrophobicity.
[0006] The second technical solution of the present invention is a method for preparing the above-mentioned FeNiCo-NC micro-nano material, which specifically comprises the following steps: (1) Dissolve iron salt, nickel salt, zinc salt and 2-methylimidazole in water and stir at room temperature for 2 h. Centrifuge, wash and dry the solution precipitate to obtain FeNi-ZIF8 precursor.
[0007] (2) FeNi-ZIF8 is placed in a cobalt salt aqueous solution, the solution is stirred at room temperature for 10-80 min, the solution precipitate is centrifuged, washed and dried to obtain a FeNiCo-ZIF8 precursor.
[0008] (3) FeNiCo-ZIF8 and dicyandiamide were loaded into two corundum boats in a mass ratio of 1:1-1.5, and pyrolyzed at 800-1000 °C under argon for 1-3 h to obtain FeNiCo-NC.
[0009] The iron salt is ferric chloride, ferric nitrate or ferric acetate; the nickel salt is nickel nitrate, nickel chloride or nickel acetate; the zinc salt is zinc nitrate, zinc chloride, zinc acetate or zinc sulfate; the molar ratio of Fe, Ni and Zn is 2-4:1:100-120.
[0010] In step (2), the cobalt salt is selected from cobalt chloride, cobalt nitrate, or cobalt acetate; and the concentration of the aqueous solution of the cobalt salt is 20-40 mM.
[0011] The step (3) specifically comprises: placing the FeNiCo-MOF nanosheets downstream of the tubular atmosphere furnace tube and placing dicyandiamide upstream; the inert gas is one of nitrogen, argon or helium; the annealing heating rate is 2-10°C / min, the annealing temperature is 800-1000°C, and the annealing time is 1-3h.
[0012] The third technical solution of the present invention is the application of the above-mentioned FeNiCo-NC material in the air electrode of zinc-air battery.
[0013] The fourth technical solution of the present invention is a zinc-air battery air electrode. The above-mentioned FeNiCo-NC nanocomposite material is added to a mixed solution formed by ethanol and Nafion, the volume ratio of ethanol to Nafion is 10: (0.2-4), and a catalyst ink is obtained after ultrasonic mixing. The catalyst ink is coated on carbon paper or carbon cloth, and dried to obtain a zinc-air battery air electrode.
[0014] A fifth technical solution of the present invention is a quasi-solid-state zinc-air battery anode material which is one of in-situ electroplated zinc materials such as zinc sheet, zinc foil, zinc strip, carbon cloth, carbon paper, etc.
[0015] The sixth technical solution of the present invention is that a gel electrolyte material of a quasi-solid-state zinc-air battery is one of a PVA electrolyte, a PANA electrolyte, a biocellulose membrane electrolyte, and an acrylic gel electrolyte.
[0016] The seventh technical solution of the present invention is a liquid zinc-air battery, which is obtained by assembling a carbon paper cathode coated with FeNiCo-NC nanomaterials, a zinc anode electrode, and a potassium hydroxide zinc acetate electrolyte.
[0017] The eighth technical solution of the present invention is a quasi-solid-state zinc-air battery, which is obtained by assembling a carbon paper cathode coated with FeNiCo-NC nanomaterials, a zinc anode electrode, and a gel electrolyte.
[0018] Compared with the prior art, the present invention has the following beneficial effects: The FeNiCo-NC catalyst material preparation process of the present invention uses cheap water as a solvent instead of methanol, and the entire preparation process is low-cost and time-saving. The FeNiCo-NC catalyst material is a multiphase metal catalyst of iron particles, nickel-iron alloy and cobalt-iron alloy supported on a carbon substrate. Compared with other metal particle catalysts, its ORR and OER bifunctional activities are higher. In addition, the FeNiCo-NC material has a composite structure in which carbon nanotubes are in situ grown on a three-dimensional carbon skeleton. This structure is similar to the surface of a fly covered with bristles and has good hydrophobicity. This hydrophobic structure can isolate some water molecules in the electrolyte, allowing more air to diffuse to the catalyst chemical reaction interface, thereby improving the power density of the zinc-air battery. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 It is the XRD pattern of the products prepared in Examples 1, 2 and 3, wherein: the abscissa X is the diffraction angle (2θ), and the ordinate Y is the relative diffraction intensity.
[0020] Figure 2 The SEM images of the products prepared in Examples 1, 2, and 3 (5 μm and 500 nm) are shown below: Figure 3 is the hydrophobic contact angle of the materials prepared in Examples 1, 2, and 3.
[0021] Figure 4 It is the ORR performance diagram of the materials prepared in Examples 1, 2, and 3.
[0022] Figure 5 This is the ORR stability test performance diagram of the FeNiCo-NC material prepared in Example 3.
[0023] Figure 6 This is the OER performance diagram of the FeNiCo-NC material prepared in Example 3.
[0024] Figure 7 This is the OER stability test performance diagram of the FeNiCo-NC material prepared in Example 3.
[0025] Figure 8 This is the open circuit voltage diagram of the FeNiCo-NC liquid zinc-air battery in Example 4.
[0026] Fig. 9 is the power density of the FeNiCo-NC liquid zinc-air battery in Example 4.
[0027] Fig.10 This is the cycle performance result of the FeNiCo-NC liquid zinc-air battery in Example 4.
[0028] Fig.11 This is the open circuit voltage diagram of the FeNiCo-NC quasi-solid-state zinc-air battery in Example 5.
[0029] Fig.12 is the power density of the FeNiCo-NC quasi-solid-state zinc-air battery in Example 5.
[0030] Fig.13 This is the cycling performance result of the FeNiCo-NC quasi-solid-state zinc-air battery in Example 5.
[0031] Fig.14 This is a picture of the FeNiCo-NC quasi-solid-state zinc-air battery lighting up an LED lamp in Example 5. DETAILED DESCRIPTION
[0032] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0033] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0034] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0035] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0036] Example 1 An iron-nickel metal particle catalyst for a zinc-air battery, the preparation method of which comprises the following steps: 96mmol 2-methylimidazole, 12mmol Zn(NO 3 ) 2 6H 2 O, 2mmol Fe(NO 3 ) 3 9H 2 O and 1mmolNi(NO 3 ) 2 6H 2 O was dissolved in aqueous solution and stirred at room temperature for 2 h. The solution precipitate was centrifuged, washed and dried to obtain FeNi-ZIF8 precursor. 1 g of FeNi-ZIF8 was placed in a corundum boat and placed in the center of a tube furnace. It was pyrolyzed at 900 °C under argon for 2 h to obtain FeNi-NC-1.
[0037] Example 2 An iron-nickel metal particle catalyst for a zinc-air battery, the preparation method of which comprises the following steps: 96mmol 2-methylimidazole, 12mmol Zn(NO 3 ) 2 6H 2 O, 2mmol Fe(NO 3 ) 3 9H 2 O and 1mmolNi(NO 3 ) 2 6H 2 O was dissolved in the aqueous solution and stirred at room temperature for 2 h. The solution precipitate was centrifuged, washed and dried to obtain FeNi-ZIF8 precursor. 1 g of FeNi-ZIF8 was loaded into corundum boat A and placed in the center of the tube furnace. 1.5 g of dicyandiamide was loaded into corundum boat B and placed on the left side of corundum boat A and close to it. It was pyrolyzed at 900 ° C under argon for 2 h to obtain FeNi-NC-2.
[0038] Example 3 An iron-cobalt-nickel metal particle catalyst for a zinc-air battery, the preparation method of which comprises the following steps: 96mmol 2-methylimidazole, 12mmol Zn(NO 3 ) 2 6H 2 O, 2mmol Fe(NO 3 ) 3 9H 2 O and 1mmolNi(NO 3 ) 2 6H 2O was dissolved in an aqueous solution and stirred at room temperature for 2 hours. The solution precipitate was centrifuged, washed and dried to obtain a FeNi-ZIF8 precursor. 1g of FeNi-ZIF8 was placed in a 40mM cobalt nitrate aqueous solution and dispersed under ultrasonic conditions for 2 minutes. The solution was stirred at room temperature for ion exchange, and the solution precipitate was centrifuged to obtain a FeNiCo-ZIF8 precursor. 1g of FeNiCo-ZIF8 was loaded into a corundum boat A and placed in the center of a tube furnace. 1.5g of dicyandiamide was loaded into a corundum boat B and placed on the left side of the corundum boat A and close to it. It was pyrolyzed at 900℃ under argon for 2 hours to obtain FeNiCo-NC.
[0039] Example 4 A liquid zinc-air battery based on FeNiCo-NC catalyst: 10 mg FeNiCo-NC, 2 ml ethanol and Nafion were prepared into a solution (the volume ratio of ethanol to Nafion was 10:0.2~4), and the solution was evenly dispersed by ultrasonic. 0.4 ml of the above solution was dropped on carbon paper and dried at 50°C as the cathode, and the pure zinc sheet was used as the anode. The cathode and anode were assembled together using a liquid zinc-air battery mold, and 6 M KOH+0.2 M (CH3COO) was added into the battery. 2 Zn solution to obtain FeNiCo-NC liquid zinc-air battery.
[0040] Example 5 A quasi-solid-state zinc-air battery based on FeNiCo-NC catalyst: 10 mg FeNiCo-NC, 2 ml ethanol and Nafion were prepared into a solution (the volume ratio of ethanol to Nafion was 10:0.2~4), and the solution was evenly dispersed by ultrasonic. 0.4 ml of the above solution was dropped on carbon paper and dried at 50°C as the cathode, and the pure zinc sheet was used as the anode. The cathode and the anode were separated by PANA electrolyte, and the three were fixed to obtain the FeNiCo-NC quasi-solid-state zinc-air battery.
[0041] Analysis of the attached figure: Figure 1 The XRD phases of Examples 1, 2, and 3 are shown in Table 1. Examples 1 and 2 contain Fe, Fe 0.5 Ni 0.5 , Example 3 contains Fe, Fe 0.5 Ni 0.5and CoFe. The broad diffraction peak between 20° and 30° corresponds to the characteristic structure of carbon (C PDF#00-041-1487). By comparison, it can be found that the crystallinity of the carbon peak of Example 2 annealed with dicyandiamide is stronger than that of Example 1; the crystallinity of the carbon peak of Example 3 annealed with dicyandiamide while adding metallic cobalt is stronger than that of Example 2. This shows that dicyandiamide annealing can enhance the graphitization degree of carbon, and the CoFe alloy produced by adding metallic cobalt can further enhance the graphitization degree of carbon materials. The enhanced graphitization degree of carbon can improve the conductivity of carbon materials, which is beneficial to the transmission of electrons in ORR and OER reactions.
[0042] Figure 2 These are scanned images of Examples 1, 2, and 3 (5 μm and 500 nm). Figure 2 a and b show the structure of Example 1, which is metal particles loaded on broken porous carbon. Figure 2 c and d show the structure of metal particles loaded on porous carbon in Example 2. From the enlarged view, it can be seen that there are a small amount of carbon nanotubes inside the carbon matrix, indicating that the use of dicyandiamide can catalyze the growth of carbon nanotubes. Figure 2 e and 2f show the hierarchical structure of the in-situ grown carbon nanotubes on the carbon substrate in Example 3. The reason is that FeNi-ZIF8 placed in cobalt nitrate will adsorb cobalt ions on the surface. During annealing, these cobalt ions are reduced and combined with the iron ions contained in FeNi-ZIF8 to form CoFe alloy, which further catalyzes the growth of carbon nanotubes.
[0043] Figure 3 The hydrophobic angles of Examples 1, 2, and 3 are 138.84°, 138.53°, and 150.38°, respectively. It can be found that the FeNiCo-NC material described in Example 3 has super hydrophobicity, which is attributed to the fact that the FeNiCo-NC material of Example 1 has a hierarchical structure of carbon nanotubes grown on a carbon substrate and has good hydrophobicity. However, there are no carbon nanotubes in the FeNi-NC-1 of Example 1, and the FeNi-NC-2 carbon nanotubes of Example 2 are wrapped in a carbon substrate and do not have such a hierarchical structure, so their hydrophobicity is poor.
[0044] Figure 4 The FeNi-NC-1 sample of Example 1 (Eonset=0.973V, E 1 / 2 =0.87V) ORR performance is average. The FeNi-NC-2 sample of Example 2 obtained by annealing with dicyandiamide shows a more positive onset potential (Eonset = 1.02V) and half-wave potential (E 1 / 2=0.912V, indicating that the assisted pyrolysis of dicyandiamide is the key to improving its ORR performance. 1 / 2 =0.87V) also has excellent oxygen reduction performance, which is slightly lower than that of FeNi-NC-2 by 4 and 3mV, but it has acquired superhydrophobic properties, which promotes the ORR reaction.
[0045] Figure 5 The chronoamperometry method was used to continuously discharge for 7200 s at a voltage of -0.4 V. The stability of the FeNiCo-NC material of Example 3 was tested, and its current retention rate was 96%, indicating that it had good stability.
[0046] Figure 6 The FeNiCo-NC catalyst of Example 3 was tested at 10 mA cm −2 The OER catalytic performance of FeNi-NC-1 of Example 1 and FeNi-NC-2 of Example 2 was poor, which were 380 and 350 mV, respectively.
[0047] Figure 7 The hourly current curve of the FeNiCo-NC catalyst loaded with Example 3 and continuously operated at 1.55 V vsRHE for 24 h in 1 M KOH electrolyte has a current retention rate of 96%, indicating that it has good OER stability.
[0048] Figure 8 , 9 , 10 showed that the liquid zinc-air battery assembled from FeNiCo-NC material has a high open circuit voltage of 1.58 V and a peak power density of up to 239 mW cm 2 , continuous charge and discharge cycle can reach 4000 hours.
[0049] Fig.11 , 12 , 13 showed that the quasi-solid-state zinc-air battery assembled from FeNiCo-NC materials has an open circuit voltage of 1.49 V and a peak power density of up to 602 mW cm 2 , the continuous charge and discharge cycle can reach 250 cycles.
[0050] Fig.14 Two quasi-solid-state zinc-air batteries assembled from the FeNiCo-NC material prepared in Example 4 connected in series can easily light up an LED lamp.
Claims
1. A method for preparing FeNiCo-NC micro-nano materials, It is characterized in that The following steps are involved: (1) Preparation of FeNi-ZIF8 nanosheets: An aqueous solution of iron salt, nickel salt, zinc salt and 2-methylimidazole was stirred at room temperature and then centrifuged, washed and dried to obtain FeNi-ZIF8; (2) Preparation of FeNiCo-ZIF8: FeNi-ZIF8 is immersed in an aqueous solution of a cobalt salt, and then centrifuged, cleaned, and dried to obtain FeNiCo-ZIF8; (3) Preparation of FeNiCo-NC: FeNiCo-ZIF8 was pyrolyzed with the assistance of dicyandiamide and annealed under inert atmosphere to obtain FeNiCo-NC.
2. The method for preparing the FeNiCo-NC micro-nano material according to claim 1, It is characterized in that In the step (1), the iron salt is ferric chloride, ferric nitrate, or ferric acetate; the nickel salt is nickel nitrate, nickel chloride, or nickel acetate; the zinc salt is zinc nitrate, zinc chloride, zinc acetate, or zinc sulfate; and the molar ratio of Fe, Ni, and Zn is 2-4:1:100-120.
3. The method for preparing the FeNiCo-NC micro-nano material according to claim 1, It is characterized in that In step (2), the cobalt salt is selected from cobalt chloride, cobalt nitrate, or cobalt acetate; and the concentration of the aqueous solution of the cobalt salt is 20-40 mM.
4. The method for preparing the FeNiCo-NC micro-nano material according to claim 1, It is characterized in that The step (3) specifically comprises: placing the FeNiCo-ZIF8 nanosheets downstream of the tubular atmosphere furnace tube and placing dicyandiamide upstream; the inert gas is one of nitrogen, argon or helium; the annealing heating rate is 2-10°C / min, the annealing temperature is 800-1000°C, and the annealing time is 1-3h.
5. Air cathode of liquid zinc-air battery or quasi-solid zinc-air battery, It is characterized in that The invention comprises a FeNiCo-NC micro-nano material prepared by the method according to any one of claims 1 to 4.
6. The air cathode of the liquid zinc-air battery or quasi-solid zinc-air battery according to claim 5, It is characterized in that The FeNiCo-NC micro-nano material prepared by the method according to any one of claims 1 to 4 is prepared into a solution according to the ratio of FeNiCo-NC, ethanol and Nafion, the solution is evenly dispersed by ultrasonication and then dripped onto carbon paper, and dried to obtain an air cathode.
7. A liquid zinc-air battery, comprising the air cathode according to claim 5 or 6, a zinc anode, and a liquid zinc-air battery composed of potassium hydroxide + zinc acetate electrolyte.
8. The liquid zinc-air battery according to claim 7, It is characterized in that The zinc anode is selected from one of zinc sheet, zinc foil and zinc powder.
9. A quasi-solid-state zinc-air battery, comprising the air cathode according to claim 5 or 6, a zinc anode, and a gel electrolyte.
10. The quasi-solid-state zinc-air battery according to claim 9, It is characterized in that The zinc anode is selected from one of zinc sheet, zinc foil and zinc powder; the solid electrolyte material can be one of PVA electrolyte, PANA electrolyte, biocellulose membrane electrolyte and acrylic gel electrolyte.