Nickel-nitrogen-doped multi-walled carbon nanotube, preparation method and application thereof, and modified electrode

By doping nickel and nitrogen elements into multi-wall carbon nanotubes, the nickel-doped multi-wall carbon nanotubes are solved, and the electrochemical activity and chemical stability are improved. , significantly improves the detection capability and stability of the electrode.

CN118993042APending Publication Date: 2024-11-22YANCHENG DANAN ENVIRONMENTAL TESTING CO LTD +2
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
CN202411112097.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Existing electrochemical detection technologies are difficult to detect acetaminophen (APAP) and dopamine (DA) efficiently at the same time, and it is difficult to improve its electrochemical activity and chemical stability.

Method used

Ni-ni-doped multi-walled carbon nanotubes are formed by doping nickel and nitrogen into multi-walled carbon nanotubes and prepared by self-polymerization and thermal cracking methods to modify the electrodes to improve electrochemical activity and chemical stability sex.

Benefits of technology

Synchronous detection of APAP and DA is achieved, the anti-interference ability, repeatability and stability of the electrode are improved, the electrocatalytic activity and conductivity are significantly improved, and different substances can be effectively catalyzed under different potentials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993042A_ABST
    Figure CN118993042A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of modified electrodes, in particular to a nickel-nitrogen-doped multi-walled carbon nanotube, a preparation method and application thereof and a modified electrode. The invention provides a preparation method of a nickel-nitrogen-doped multi-walled carbon nanotube, which comprises the following steps: mixing a buffer solution of the multi-walled carbon nanotube with dopamine hydrochloride, and carrying out self-polymerization reaction to obtain a polydopamine-coated multi-walled carbon nanotube; and adsorbing the polydopamine-coated multi-walled carbon nanotube in a soluble nickel salt solution, and carrying out thermal cracking in an argon atmosphere to obtain the nickel-nitrogen-doped multi-walled carbon nanotube. The nickel-nitrogen-doped multi-walled carbon nanotube prepared by the preparation method can be effectively used for simultaneous detection of APAP and DA, and has relatively high electrochemical activity and chemical stability.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of modified electrodes, and in particular to a nickel-nitrogen doped multi-walled carbon nanotube and a preparation method and application thereof, and a modified electrode. Background Art

[0002] Bioactive molecules such as acetaminophen (APAP) and dopamine (DA) have similar nitrogen aromatic structures and are important for human metabolism. APAP is the most widely used analgesic in the world and is often used interchangeably with aspirin. It has a narrow safety range between effectiveness and potential toxicity. Abuse of APAP can lead to liver and kidney toxicity and may even be fatal. On the other hand, DA plays an essential role in the central nervous and renal systems. It is involved in various daily activities and is closely related to the onset and progression of many diseases. Specifically, irregular DA levels in organisms can lead to various neurodegenerative diseases, including schizophrenia and Alzheimer's disease. Therefore, accurate detection of APAP and DA is crucial for neurological and biomedical health diagnosis.

[0003] Currently, a variety of techniques can be used to detect APAP and DA, such as spectrophotometry, chromatography, electrophoresis, chemiluminescence, and electrochemical analysis. Among these methods, electrochemical technology has become a reliable method for detecting target substances with high sensitivity, rapidity, simplicity, and low cost. However, it may be challenging to achieve simultaneous detection of the two substances and to simultaneously improve their electrochemical activity and chemical stability, and optimizing the structure of electrode materials is crucial. Summary of the invention

[0004] The purpose of the present invention is to provide a nickel-nitrogen doped multi-walled carbon nanotube and a preparation method and application thereof, and a modified electrode. The nickel-nitrogen doped multi-walled carbon nanotube prepared by the preparation method can be effectively used for the simultaneous detection of APAP and DA, and has high electrochemical activity and chemical stability.

[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0006] The invention provides a nickel-nitrogen doped multi-walled carbon nanotube, comprising a multi-walled carbon nanotube and nickel elements and nitrogen elements doped in the multi-walled carbon nanotube.

[0007] Preferably, the nickel doping amount in the nickel-nitrogen doped multi-walled carbon nanotubes is 0.5 at.% to 3 at.%, and the nitrogen doping amount is 0.5 at.% to 4 at.%;

[0008] The outer diameter of the nickel-nitrogen doped multi-walled carbon nanotube is 5-25 nm.

[0009] The present invention also provides a method for preparing nickel-nitrogen doped multi-walled carbon nanotubes as described in the above technical solution, comprising the following steps:

[0010] The buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride are mixed to carry out a self-polymerization reaction to obtain multi-walled carbon nanotubes coated with polydopamine;

[0011] The multi-walled carbon nanotubes coated with polydopamine are adsorbed in a soluble nickel salt solution and then thermally cracked in an argon atmosphere to obtain the nickel-nitrogen doped multi-walled carbon nanotubes.

[0012] Preferably, the concentration of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer is 0.2 to 5 mg / mL;

[0013] The solvent in the buffer of the multi-walled carbon nanotubes is Tris buffer.

[0014] Preferably, the mass ratio of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer to the dopamine hydrochloride is (1-5): (1-5).

[0015] Preferably, the pH of the mixed solution obtained after the mixing is 6-11.

[0016] Preferably, the amount ratio of the polydopamine-coated multi-walled carbon nanotubes to the soluble nickel salt solution is (1-5) mg: (1-5) mL;

[0017] The concentration of the soluble nickel salt solution is 5-20 mol / L.

[0018] Preferably, the annealing temperature is 500-1000° C. and the time is 1-5 hours.

[0019] The present invention also provides the use of the nickel-nitrogen doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution in preparing modified electrodes.

[0020] The present invention also provides a modified electrode, comprising an electrode and nickel-nitrogen doped multi-walled carbon nanotubes coated on the surface of the electrode;

[0021] The nickel-nitrogen doped multi-walled carbon nanotubes are the nickel-nitrogen doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution.

[0022] The present invention provides a nickel-nitrogen doped multi-walled carbon nanotube, comprising a multi-walled carbon nanotube and a nickel element and a nitrogen element doped in the multi-walled carbon nanotube. The present invention introduces nitrogen atoms into the multi-walled carbon nanotube, so that the lone pair of electrons on the nitrogen atom can be combined with the multi-walled carbon nanotube, resulting in more positional defects, thereby improving the electrochemical activity and chemical stability; on the other hand, the multi-walled carbon nanotube doped with nitrogen can be used as a catalytic substrate for loading active nanoparticles, adding active sites based on an interwoven network structure, and utilizing the strong activity, stability and low cost of nickel to improve the activity of the material. Therefore, the present invention uses DA as a unit and a soluble nickel salt as a metal source, and significantly improves the electrocatalytic activity and conductivity of the material by introducing nickel and nitrogen into the multi-walled carbon nanotube. Then improve the anti-interference ability, good repeatability and stability of the modified electrode; at the same time, the nickel-nitrogen doped multi-walled carbon nanotube can realize the synchronous catalysis of different substances at different potentials, and can be effectively used to simultaneously detect APAP and DA in actual samples. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] Figure 1 Schematic diagram of the preparation process of nickel-nitrogen doped multi-walled carbon nanotubes in an embodiment of the present invention;

[0024] Figure 2 The results of the modified electrodes described in Examples 2 to 7 detecting 200.0 μM APAP solution and 30.0 μM DA solution;

[0025] Figure 3 The SEM, TEM, HRTEM-EDS, XRD and XPS images of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1;

[0026] Figure 4 The SEM images of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1 at different regions and different magnifications;

[0027] Figure 5 The atomic percentage composition of various elements in the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1;

[0028] Figure 6 The Raman spectra of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2 are shown in FIG. D and I G Strength ratio;

[0029] Figure 7 The XPS full spectrum of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1 (a) and (c) 1s High-resolution XPS spectrum of (b);

[0030] Figure 8 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, the MWCNTs-GCE prepared in Comparative Example 3, the Ni / NiC X -N-MWCNTs-GCE and bare GCE were in a 0.1MPB solution consisting of 200.0 μM APAP solution and 5.0 mM [Fe(CN)6] 3- / 4- CV curves in solution and in 0.1 M PB solution composed of 50.0 μM DA solution and 5.0 mM [Fe(CN)6] 3- / 4- CV curves in solution;

[0031] Fig. 9 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, the Ni / NiC described in Example 5 X -N-MWCNTs-GCE and bare GCE were exposed to 5.0 mM Fe(CN)6 3- / 4- EIS graph in (1:1);

[0032] Fig.10 In PB solution (pH 7.0), the Ni / NiC X -N-MWCNT-GCE modified electrode obtained APAP (a) and DA (b) CV curves at different scan rates; APAP (c) and DA (d) SWV curves in 0.1M PB at different pH values ​​under Ni / NiCX-N-MWCNTs / GCE; Effect of pH value on the oxidation peak current and peak potential of APAP (e) and DA (f);

[0033] Fig.11 Linear fits of the peak current of APAP (a) and DA (b) versus the square root of the scan rate, and the relationship between the peak potential of APAP (c) and DA (d) and the natural logarithm of the scan rate.

[0034] Fig.12 Figure 2 is the current response curves of different APAP concentrations (a) and the linear curve of APAP (b) in a system with 50 μM DA; the current response curves of different DA concentrations (c) and the linear curve of DA (d) in a system containing 50.0 μM APAP; the Ni / NiC X-N-MWCNT-GCE modified electrode APAP and DA (e) change of current response curve and APAP and DA (f) linear curve; Example 5 Ni / NiC X -I t curves of the N-MWCNT-GCE modified electrode (g) for sequential addition of APAP aminophenol and impurities in PB (impurities ak correspond to APAP, DA, MgCl2, CuNO3, KCl, FeCl2, Na2SO4, glucose, L-tyrosine, and glycine, respectively); reproducibility (h) and repeatability (i) test bar graphs. DETAILED DESCRIPTION

[0035] The invention provides a nickel-nitrogen doped multi-walled carbon nanotube, comprising a multi-walled carbon nanotube and nickel elements and nitrogen elements doped in the multi-walled carbon nanotube.

[0036] In the present invention, the nickel doping amount in the nickel-nitrogen doped multi-walled carbon nanotubes is preferably 0.5at.% to 3at.%, more preferably 1.5at.% to 2.5at.%, and most preferably 2.07at.%; the nitrogen doping amount is preferably 0.5at.% to 4at.%, more preferably 1at.% to 2at.%, and most preferably 1.71at.%.

[0037] In the present invention, the outer diameter of the nickel-nitrogen doped multi-walled carbon nanotubes is preferably 5 to 25 nm, more preferably 7 to 20 nm.

[0038] The present invention also provides a method for preparing nickel-nitrogen doped multi-walled carbon nanotubes as described in the above technical solution, comprising the following steps:

[0039] The buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride are mixed to carry out a self-polymerization reaction to obtain multi-walled carbon nanotubes coated with polydopamine;

[0040] The multi-walled carbon nanotubes coated with polydopamine are adsorbed in a soluble nickel salt solution and then thermally cracked in an argon atmosphere to obtain the nickel-nitrogen doped multi-walled carbon nanotubes.

[0041] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0042] The invention mixes a buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride to carry out a self-polymerization reaction to obtain multi-walled carbon nanotubes coated with polydopamine.

[0043] In the present invention, the concentration of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer is preferably 0.2-5 mg / mL, more preferably 0.5-2 mg / mL, and most preferably 1 mg / mL; the solvent in the multi-walled carbon nanotube buffer is preferably Tris buffer.

[0044] In the present invention, the mass ratio of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer to the dopamine hydrochloride is preferably (1-5):(1-5), more preferably (1-2):(1-2), and most preferably 1:1.

[0045] The present invention has no special limitation on the mixing process. The process well known to those skilled in the art is adopted to ensure that the pH of the mixed solution obtained by mixing is 6 to 11, more preferably 8 to 9, and most preferably 8.5.

[0046] In the present invention, the self-polymerization reaction is preferably carried out under ultrasonic conditions; the frequency of the ultrasound is preferably 20-200 KHz, more preferably 20-80 KHz, and most preferably 40 KHz; the time of the ultrasound is preferably 5-120 min, more preferably 5-100 min, and most preferably 10 min.

[0047] After the ultrasonic treatment is completed, the present invention also preferably includes stirring, centrifugation, washing and drying performed in sequence. In the present invention, the stirring temperature is preferably room temperature; the stirring speed is preferably 100 to 1000 rpm, more preferably 100 to 500 rpm, and most preferably 200 rpm; the stirring time is preferably 2 to 10 hours, more preferably 3 to 5 hours, and most preferably 4 hours. The present invention does not have any special restrictions on the centrifugation, washing and drying processes, and the processes well known to those skilled in the art can be used.

[0048] After obtaining the polydopamine-coated multi-walled carbon nanotubes, the present invention adsorbs the polydopamine-coated multi-walled carbon nanotubes in a soluble nickel salt solution and then performs thermal cracking in an argon atmosphere to obtain the nickel-nitrogen doped multi-walled carbon nanotubes.

[0049] The present invention has no special limitation on the type of the soluble nickel salt solution, and any type known to those skilled in the art can be used. In a specific embodiment of the present invention, the soluble nickel salt solution is specifically a nickel chloride solution.

[0050] In the present invention, the concentration of the soluble nickel salt solution is preferably 5 to 20 mmol / L, more preferably 8 to 12 mmol / L, and most preferably 10.0 mmol / L.

[0051] In the present invention, the usage ratio of the polydopamine-coated multi-walled carbon nanotubes to the soluble nickel salt solution is preferably (1-5) mg: (1-5) mL, more preferably 1 mg: (1-3) mL, and most preferably 1 mg: 2 mL.

[0052] In the present invention, the adsorption is preferably carried out under stirring conditions, and in the present invention, the adsorption time is preferably 3 to 15 hours, more preferably 6 to 10 hours, and most preferably 8 hours. The present invention does not have any special restrictions on the speed of the stirring, and a speed well known to those skilled in the art can be used to ensure that the nickel ions are uniformly adsorbed on the surface of the multi-walled carbon nanotubes.

[0053] After the adsorption is completed, the present invention also preferably includes centrifugation, washing and drying in sequence; the present invention has no special restrictions on the centrifugation and washing process, and can be carried out using a process well known to those skilled in the art. In the present invention, the drying is preferably vacuum drying; the temperature of the vacuum drying is preferably 60°C, and the present invention has no special restrictions on the time of the vacuum drying, and can be carried out using a time well known to those skilled in the art and ensuring sufficient drying.

[0054] In the present invention, the temperature of the thermal cracking is preferably 500-1000°C, more preferably 700-900°C, most preferably 800°C; the time is preferably 1-5h, more preferably 1-3h, most preferably 2h.

[0055] The present invention also provides the use of the nickel-nitrogen doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution in preparing modified electrodes.

[0056] The present invention also provides a modified electrode, comprising an electrode and nickel-nitrogen doped multi-walled carbon nanotubes coated on the surface of the electrode;

[0057] The nickel-nitrogen doped multi-walled carbon nanotubes are the nickel-nitrogen doped multi-walled carbon nanotubes described in the above technical solution or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method described in the above technical solution.

[0058] In the present invention, the method for preparing the modified electrode preferably comprises the following steps:

[0059] The nickel-nitrogen doped multi-walled carbon nanotube suspension is coated on the surface of the electrode and dried to obtain the modified electrode.

[0060] In the present invention, the concentration of the nickel-nitrogen doped multi-walled carbon nanotube suspension is preferably 0.5 mg·mL -1 In the present invention, the coating amount of the nickel-nitrogen doped multi-walled carbon nanotube suspension is preferably 4 to 9 μL.

[0061] The nickel-nitrogen doped multi-walled carbon nanotubes and their preparation method and application, and modified electrodes provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the scope of protection of the present invention.

[0062] Example 1

[0063] like Figure 1 As shown, 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes to maintain a pH of 8.5, and after ultrasonic treatment for 10 min (ultrasonic frequency of 40 KHz), the obtained mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), centrifuged, washed and dried in sequence to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA);

[0064] 50.0 mg of the MWCNTs-PDA was dispersed in 100 mL of nickel chloride solution (concentration of 10.0 mmol / L), stirred continuously (stirring speed of 200 rpm) for 8 h, centrifuged, washed and vacuum dried at 60 ° C for 12 h, and then annealed at 800 ° C for 2 h in an argon atmosphere to obtain nickel-nitrogen doped multi-walled carbon nanotubes (Ni / NiC x -N-MWCNTs).

[0065] Embodiments 2 to 7

[0066] A glassy carbon electrode (GCE electrode) was polished with alumina powders with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, and then rinsed with ultrapure water, and then ultrasonically treated in anhydrous alcohol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode;

[0067] The surface of the pretreated GCE electrode was coated with the nickel-nitrogen doped multi-walled carbon nanotube suspension (concentration 0.5 mg mL -1 The coating amount was 4 μL (Example 2), 5 μL (Example 3), 6 μL (Example 4), 7 μL (Example 5), 8 μL (Example 6) and 9 μL (Example 7) in sequence, and then dried to obtain a modified electrode (denoted as Ni / NiC X -N-MWCNTs-GCE).

[0068] Comparative Example 1

[0069] 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes to maintain a pH value of 8.5, and after ultrasonic treatment for 10 min (ultrasonic frequency of 40 KHz), the obtained mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), centrifuged, washed and dried in sequence to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA);

[0070] A glassy carbon electrode (GCE electrode) was polished with alumina powders with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, and then rinsed with ultrapure water, and then ultrasonically treated in anhydrous alcohol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode;

[0071] The MWCNTs-PDA suspension (concentration 0.5 mg mL -1 , coating amount was 7 μL), and dried to obtain a modified electrode (denoted as MWCNTs-PDA-GCE).

[0072] Comparative Example 2

[0073] Preparation of MWCNT-N-PC-GCE:

[0074] 50.0 mg of dopamine hydrochloride was dissolved in 50.0 mL of Tris buffer containing 50.0 mg of multi-walled carbon nanotubes to maintain a pH value of 8.5, and after ultrasonic treatment for 10 min (ultrasonic frequency of 40 KHz), the obtained mixture was stirred at room temperature for 4 h (stirring speed of 200 rpm), centrifuged, washed and dried in sequence to obtain polydopamine (PDA) coated multi-walled carbon nanotubes (MWCNTs-PDA);

[0075] Then, 50.0 mg of MWCNTs-PDA powder was annealed at 800 °C for 2 h (argon flow) to form MWCNT-N-PC nanostructures.

[0076] A glassy carbon electrode (GCE electrode) was polished with alumina powders with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, and then rinsed with ultrapure water, and then ultrasonically treated in anhydrous alcohol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode;

[0077] The MWCNT-N-PC suspension (concentration of 0.5 mg mL) was coated on the surface of the pretreated GCE electrode. -1 , coating amount was 7 μL), and dried to obtain a modified electrode (denoted as MWCNT-N-PC-GCE).

[0078] Comparative Example 3

[0079] Preparation of MWCNTs-GCE:

[0080] A glassy carbon electrode (GCE electrode) was polished with alumina powders with particle sizes of 1.00 μm, 0.30 μm and 0.05 μm, and then rinsed with ultrapure water, and then ultrasonically treated in anhydrous alcohol and ultrapure water, and dried at room temperature to obtain a pretreated GCE electrode;

[0081] The MWCNTs suspension (concentration of 0.5 mg mL -1 , coating amount was 7 μL), and dried to obtain a modified electrode (denoted as MWCNTs-GCE).

[0082] Test Example 1

[0083] The modified electrodes described in Examples 2 to 7 were used to detect 200.0 μM APAP solution and 30.0 μM DA solution. The detection results are as follows: Figure 2 As shown by Figure 2 It can be seen that when the coating amount of the catalyst (nickel-nitrogen doped multi-walled carbon nanotube suspension) is 7 μL (Example 5), the current change is the largest, and the simultaneous detection performance of APAP and DA is the best;

[0084] The modified electrode described in Example 5 was characterized by cyclic voltammetry (CV) and square wave voltammetry (SWV): CV measurement was performed in 10 mL of 0.1 mol / L PB solution (the test conditions for CV measurement were: in 10 mL of 0.1 mol L -1 CV measurements were performed in PB solution); SWV was performed in 0.1 mol / L phosphate buffer solution (PB, pH = 7.0) containing different concentrations of APAP (the concentrations were 0, 1, 2, 5, 10, 20, 30, 50, 80, 100, 120, 150 μM), with a potential range of 0.1-0.6 V, and the amplitude, frequency, and increment E were 0.025 V, 10 Hz, and 0.004 V, respectively;

[0085] The nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1 were subjected to SEM, TEM, HRTEM-EDS, XRD and XPS tests. The test results are as follows: Figures 3-4 As shown, Figure 3 In the figure, (a) is the SEM image of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1, (b) is the TEM image of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1, (c) to (f) are HRTEM-EDS images of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1, (g) is the XRD image of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2, (h) is the N 1s The high-resolution XPS spectrum of the nickel-nitrogen doped multi-walled carbon nanotubes is shown in FIG. 2p High-resolution XPS spectra; Figure 4The SEM images of the nickel-nitrogen doped multi-walled carbon nanotubes in different regions and at different magnifications described in Example 1, wherein (a), (d) and (g) are SEM images of the same region at different magnifications, (b), (e) and (h) are SEM images of the same region at different magnifications, and (c), (f) and (i) are SEM images of the same region at different magnifications; Figure 5 is the atomic percentage composition of various elements in the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1; Figures 3 to 5 It can be seen that the nanotubes in the nickel-nitrogen-doped multi-walled carbon nanotubes are intertwined, presenting a loose and porous macroscopic morphology. This morphology can expose more active sites, expand the specific surface area, and improve the electrocatalytic activity. At the same time, the typical morphology of multi-walled carbon nanotubes presents a relatively smooth and flat surface, and carbon nanotubes of different lengths are arranged in a staggered manner. After carbonization of PDA and nickel source, the surface becomes rough due to the formation of a carbon layer on the surface of the multi-walled carbon nanotubes, and the nanowire array remains intact. From the TEM image of the nickel-nitrogen-doped multi-walled carbon nanotubes, it can be seen that nitrogen and nickel are uniformly distributed in the internal structure of the nickel-nitrogen-doped multi-walled carbon nanotubes. The HRTEM-EDS elemental spectrum proves the coexistence and uniform distribution of C, N and Ni elements in nickel-nitrogen-doped multi-walled carbon nanotubes. The element percentages of C, N and Ni are 96.20%, 1.71% and 2.07% respectively; XRD diagrams show that for multi-walled carbon nanotubes, there are main hexagonal graphite characteristic diffraction peaks at 25.9° and 44.1°, which are respectively attributed to the (002) and (101) crystal planes of multi-walled carbon nanotubes (JCPDS No. 26-1077). It can also be seen that the hexagonal graphite characteristic peaks are still retained in MWCNTs-PDA and MWCNT-N-PC (Comparative Example 2), and the reduction in peak intensity is attributed to the polydopamine coating. It is worth noting that for nickel-nitrogen doped multi-walled carbon nanotubes, there is an additional characteristic diffraction peak at 44.5°, which is indexed to the (011) plane of Ni (JCPDS No.45-1027). More specifically, while retaining the characteristic peaks of multi-walled carbon nanotubes, the diffraction peaks at 29.4°, 36.1°, 39.9°, 43.2°, and 47.7° can be indexed as the peaks of NiCx (JCPDS No.45-0979). Therefore, these results indicate that nickel-nitrogen doped multi-walled carbon nanotubes have been successfully prepared. In addition, Raman spectroscopy is used to show the level of graphitization in carbon-based materials ( Figure 6 (a), (a) Raman spectra of the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2); two characteristic spectral lines with different chemical structures are located at 1360 and 1580 cm -1The higher peak at D of the NiN-doped MWCNTs compared to MWCNTs is indicated by the decrease in order and graphitization degree. D and I G The intensity ratio indicates the degree of graphitization of carbon materials ( Figure 6 (b), (b) is the multi-walled carbon nanotubes described in Example 1, the MWCNTs-PDA described in Example 1, the nickel-nitrogen-doped multi-walled carbon nanotubes described in Example 1, and the MWCNT-N-PC described in Comparative Example 2 D and I G The intensity ratio of I D / I G It increases from 1.43 to 1.539, and the nickel-nitrogen doped multi-walled carbon nanotubes show more defects and disordered structures, which are beneficial to provide more catalytic active centers; the XRD and EDS results are consistent with the Raman spectroscopy results;

[0086] Figure 7 The XPS full spectrum of the nickel-nitrogen doped multi-walled carbon nanotubes described in Example 1 (a) and (c) 1s The high-resolution XPS spectrum (b) of Figure 3 (h) and (i) in Figure 7 It can be seen that the peaks at 844.6, 392.6 and 279.6 eV correspond to Ni2p, N1s and C1s, confirming the existence of C, N and Ni; the high-resolution XPS Ni 2p spectrum shows a weak peak at 852.7 eV attributed to metallic Ni, and three XPS peaks at 853.5, 854.1 and 855.5 eV attributed to divalent Ni 2p3 / 2. The Ni2p3 / 2 peak at 853.5 eV can be attributed to NiCx. At the same time, the peaks at 861.8 and 873.5 eV are respectively attributed to Ni 2+ and Ni 3+ , which also proves the existence of multivalent Ni carbides, and two weak peaks corresponding to the satellite peaks of metallic Ni are also observed at 878.6 and 858.1eV. In addition, characteristic peaks of carbon-carbon double bond (284.1eV), N-2p2C (284.6eV) and N-2p3C (288.3eV) are observed in the high-resolution deconvoluted C1s spectrum; in addition, the deconvoluted N1s spectrum shows three peaks at 398.3, 400.4 and 402.9eV, which are connected to pyridinic N, pyrrolic N and graphitic N, respectively, indicating that N is successfully doped in carbon materials. XPS results show that the nanohybrid contains metallic Ni and NC materials, which further confirms the correctness of the XRD and EDS spectrum results.

[0087] Test Example 2

[0088] Cyclic voltammetry (CV) and electrochemical impedance spectroscopy (EIS) were used to analyze the different modified electrodes (MWCNTs-PDA-GCE described in Comparative Example 1, MWCNT-N-PC-GCE described in Comparative Example 2, MWCNTs-GCE prepared in Comparative Example 3, Ni / NiC X -N-MWCNTs-GCE and bare GCE) were in a 0.1 M PB solution consisting of 200.0 μM APAP solution and 50.0 μM DA solution and 5.0 mM [Fe(CN)6] 3- / 4- CV curve in solution, test results are as follows Figure 8 As shown, (a) is a 0.1M PB solution composed of 200.0μM APAP solution and 5.0mM [Fe(CN)6] containing 0.1M KCl 3- / 4- CV curves in solution, (b) 0.1 M PB solution composed of 50.0 μM DA solution and 5.0 mM [Fe(CN)6] 3- / 4- CV curve in solution; Figure 8 It can be seen that Ni / NiC X -The redox peak of N-MWCNTs is significantly higher than that of other electrodes, indicating that it has more efficient electron transfer ability; Fig. 9 The MWCNTs-PDA-GCE described in Comparative Example 1, the MWCNT-N-PC-GCE described in Comparative Example 2, the Ni / NiC described in Example 5 X -N-MWCNTs-GCE and bare GCE were exposed to 5.0 mM Fe(CN)6 3- / 4- The EIS graph in (1:1) (frequency range from 100kHz to 0.1Hz, initial voltage value of 0.22V, amplitude of 0.005V) is given by Fig. 9 It can be seen that the EIS spectrum consists of two parts: a high-frequency semicircle symbolizing the constrained electron transfer process and a low-frequency linear region representing the diffusion-limited process. In the EIS graph, MWCNTs-N-PC-GCE has no clear semicircle in the high-frequency region, which indicates a high charge transfer resistance. However, in the high-frequency region, there are obvious semicircles for bare GCE, MWCNTs, and MWCNTs PDA, which are much larger than those for the fitted Ni / NiC X -N-MWCNTs equivalent circuit obtained Rct value of 75Ω, indicating that Ni / NiC X -N-MWCNTs have excellent electrocatalytic behavior;

[0089] Fig.10 In PB solution (pH 7.0), the coating volume was 7.0 μL (concentration was 0.5 mg mL-1 ) of Ni / NiC X CV curves of APAP (a) and DA (b) obtained at different scan rates on Ni / NiCX-N-MWCNT-GCE modified electrode; SWV curves of APAP (c) and DA (d) under Ni / NiCX-N-MWCNTs / GCE in 0.1M PB at different pH values; Effect of pH value on the oxidation peak current and peak potential of APAP (e) and DA (f); Fig.10 It can be seen that when 100.0 μM APAP or DA is present in PB (pH = 7.0), the CV of the scan rate varies between 5 and 10 mV / s to reflect the interface control factor. It can be clearly observed that the peak current increases with the increase in scan rate, and the oxidation and reduction peaks slightly shift to the corresponding potentials during this process. The redox peak current shows a linear correlation with the square root of the scan rate (e.g. Fig.11 (a) and (b) in the figure), and followed by the linear regression equation (as shown in equations 1 to 4);

[0090] I pa (APAP)(μA)=3.42ν 1 / 2 (mV / s)-6.92(R=0.9989) Formula 1,

[0091] I pc (APAP)(μA)=-2.24ν 1 / 2 (mV / s)+5.04(R=0.9965) Formula 2,

[0092] I pa (DA)(μA)=0.54ν 1 / 2 (mV / s)+0.012(R=0.9964) Formula 3,

[0093] I pc (DA)(μA)=-1.08ν 1 / 2 (mV / s)+1.22(R=0.9978) Formula 4;

[0094] Among them, I pa is the peak anode current, I pc is the peak cathode current, and v is the scan rate (mV / s).

[0095] The good linear relationship above indicates that the electrooxidation of APAP or DA on the modified electrode is a representative diffusion-controlled process. The correlation between the peak potential of APAP and DA and the logarithm of the scan rate is shown in Fig.11 As shown in (c) and (d) in the figure, the linear fitting equation is:

[0096] Epa (APAP)(V)=0.015lnν(mV / s)+0.36(R=0.9996) Formula 5,

[0097] E pc (APAP)(V)=-0.0092lnν(mV / s)+0.38(R=0.9969) Formula 6,

[0098] E pa (DA)(V)=0.013lnν(mV / s)+0.19(R=0.9899) Formula 7,

[0099] E pc (DA)(V)=-0.013lnν(mV / s)+0.18(R=0.9956) Formula 8,

[0100] The electron transfer coefficient (ɑ) and the electron transfer number (n) can be calculated by the Laviron equation as shown in equations 9 and 10:

[0101]

[0102] Where R, T and F represent the molar gas constant, thermodynamic temperature and Faraday constant, respectively. According to the slope of Ep versus ln, it can be calculated that the n of the electrooxidation of APAP and DA under Ni / NiCX-n-MWCNTs / GCE is about 2, indicating that under Ni / NiC X The electrode processes of APAP and DA on n-MWCNTs / GCE are reversible, which is consistent with Fig.10 The CV curves of APAP and DA in (a) and (b) are consistent. Based on this result, we derived the oxidation mechanism of APAP and DA, as shown in Eq. 11.

[0103]

[0104] Fig.10 (c) and (d) are the test results of square wave stripping voltammetry (SWV) in PB solution with a pH range of 5.0 to 9.0. From the above results, it can be seen that the increased voltage is 0.004V, the amplitude is 0.025V, and the frequency is 10Hz. When the pH is 7.0, the peak current reaches the maximum value; Fig.10 (e) and (f) are the peak potential and current fitting of pH. From the above results, it can be seen that with the increase of pH value, Ep moves to a low potential, indicating that protons participate in the electrochemical reaction. The linear regression equation between Ep and pH value is fitted as Equations 12 to 13:

[0105] Ep(APAP) / V=-0.0532pH+0.7484(R=0.9992) Formula 12,

[0106] Ep(DA) / V=-0.0576pH+0.5765(R=0.9963) Formula 13;

[0107] The absolute values ​​of their slopes (-53.2 mV / pH and -57.6 mV / pH, respectively) are in good agreement with the theoretical value of -59 mV / pH, indicating the balance of electrons and protons in the redox reaction. The figure shows that the current value first increases steadily with increasing pH, then decreases, reaching a maximum value at pH 7.0. In addition, the peak potential decreases with the continued increase in pH level. The results show that H+ participates in the reaction during the electrochemical determination process;

[0108] Fig.12 Figure 2 is the current response curves of different APAP concentrations (a) and the linear curve of APAP (b) in a system with 50 μM DA; the current response curves of different DA concentrations (c) and the linear curve of DA (d) in a system containing 50.0 μM APAP; the Ni / NiC X -N-MWCNT-GCE modified electrode APAP and DA (e) change of current response curve and APAP and DA (f) linear curve; Example 5 Ni / NiC X -The current it curve (g) of the N-MWCNT-GCE modified electrode, used for sequential addition of APAP aminophenol and impurities in PB (impurities ak correspond to APAP, DA, magnesium chloride, copper nitrate, potassium chloride, ferric chloride, sodium sulfate, glucose, L-tyrosine, and glycine, respectively); reproducibility (h) and repeatability (i) test bar graphs; from (a), it can be seen that when the concentration of one substance is kept constant and the concentration of another substance is continuously changed, when the DA concentration is kept at 50 μmol / L, the peak current of APAP increases linearly with the increase in concentration; from (b), it can be seen that the peak current of APAP is linearly related to the concentration in the range of 1 to 150 μmol / L. The linear regression equation is shown in Equation 14:

[0109] I p (APAP)(μA)=0.2236C / μM+1.1617(R=0.9969) Formula 14;

[0110] From (c) and (d), it can be seen that when the APAP concentration is kept at a certain level (1-150 μmol / L), the peak current of DA is also linearly related to the concentration. The regression equation in the range of 0-80 μmol / L is shown in Equation 15:

[0111] I p (DA)(μA)=0.7420C / μM+1.6320(R=0.9928) Formula 15;

[0112] As shown in (e), as the concentrations of the two target molecules (APAP and DA) increase, the peak responses of APAP and DA can be detected simultaneously;

[0113] From (f), it can be seen that the peak responses of APAP and DA in the range of 1-150 μmol / L show a good linear relationship, and the regression equations are shown in Equations 16-17:

[0114] I p (APAP)(μA)=0.2418C / μM-0.2383(R=0.9994) Formula 16

[0115] I p (DA)(μA)=0.7146C / μM+2.6486(R=0.9983) Formula 17;

[0116] The limit of detection (LOD) is given by the slope (M) of the calibration curve, as shown in Equation 18:

[0117] LOD = 3S / M Formula 18;

[0118] Where S is the standard deviation of the blank amperometric signal, and the detection limits of APAP and DA are 0.56 and 0.19 μmol / L, respectively (S / N=3). The results show that compared with some reported sensors for detecting APAP and DA, nickel-nitrogen-doped multi-walled carbon nanotubes have good selectivity in detecting APAP or DA, and perform well in terms of detection range and detection limit;

[0119] As shown in (g), even if the concentrations of interfering substances such as p-aminophenol, dopamine, magnesium chloride, copper nitrate, potassium chloride, ferric chloride, sodium sulfate, glucose, L-tyrosine and glycine were 100 times higher than that of APAP, the current response remained unchanged after adding the above interfering substances every 50 seconds between two additions of APAP, which means that the electrode modified with nickel-nitrogen doped multi-walled carbon nanotubes has excellent selectivity and anti-interference ability for trace detection of APAP and DA;

[0120] As shown in (h), the peak current value of the electrode modified with nickel-nitrogen-doped multi-walled carbon nanotubes can maintain 90.66% of the original peak current value after being stored at room temperature for 7 days, which shows good stability.

[0121] From (i), it can be seen that the relative standard deviation (RSD) of the nickel-nitrogen doped multi-walled carbon nanotube modified electrode is 2.01%, indicating that the nickel-nitrogen doped multi-walled carbon nanotube modified electrode has good repeatability.

[0122] In summary, the nickel-nitrogen doped multi-walled carbon nanotube modified electrode has excellent stability, repeatability and selectivity;

[0123] The electrode modified with nickel-nitrogen doped multi-walled carbon nanotubes was used to detect APAP and DA in acetaminophen tablets and dopamine injection, wherein the actual contents of acetaminophen tablets and dopamine injection were 10.0, 20.0 and 50.0 μM, respectively. The test results are shown in Table 2: The difference between the content detected by the electrode modified with nickel-nitrogen doped multi-walled carbon nanotubes and the actual content is small, the recovery rate can reach 94.85% to 110.20%, and the relative standard deviation is between 1.35% and 4.88%. It shows that the modified electrode can be effectively used for the simultaneous detection of APAP and DA, and has practical application potential.

[0124] Table 2 Actual content determination of APAP and dopamine in acetaminophen tablets and dopamine injection

[0125]

[0126]

[0127] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A nickel-nitrogen doped multi-walled carbon nanotube, It is characterized in that The invention comprises multi-walled carbon nanotubes and nickel elements and nitrogen elements doped in the multi-walled carbon nanotubes.

2. The nickel-nitrogen doped multi-walled carbon nanotube according to claim 1, It is characterized in that The nickel doping amount in the nickel-nitrogen doped multi-walled carbon nanotubes is 0.5 at.% to 3 at.%, and the nitrogen doping amount is 0.5 at.% to 4 at.%; The outer diameter of the nickel-nitrogen doped multi-walled carbon nanotube is 5-25 nm.

3. The method for preparing nickel-nitrogen doped multi-walled carbon nanotubes according to claim 1 or 2, It is characterized in that The following steps are involved: The buffer solution of multi-walled carbon nanotubes and dopamine hydrochloride are mixed to carry out a self-polymerization reaction to obtain multi-walled carbon nanotubes coated with polydopamine; The multi-walled carbon nanotubes coated with polydopamine are adsorbed in a soluble nickel salt solution and then thermally cracked in an argon atmosphere to obtain the nickel-nitrogen doped multi-walled carbon nanotubes.

4. The preparation method according to claim 3, It is characterized in that The concentration of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer is 0.2 to 5 mg / mL; The solvent in the buffer of the multi-walled carbon nanotubes is Tris buffer.

5. The preparation method according to claim 3, It is characterized in that The mass ratio of the multi-walled carbon nanotubes in the multi-walled carbon nanotube buffer to the dopamine hydrochloride is (1-5): (1-5).

6. The preparation method according to claim 3, It is characterized in that The pH of the mixed solution obtained after the mixing is 6-11.

7. The preparation method according to claim 3, It is characterized in that The polydopamine-coated multi-walled carbon nanotubes and the soluble nickel salt solution are used in a ratio of (1-5) mg: (1-5) mL; The concentration of the soluble nickel salt solution is 5-20 mol / L.

8. The preparation method according to claim 3, It is characterized in that The annealing temperature is 500-1000° C. and the annealing time is 1-5 hours.

9. Use of the nickel-nitrogen doped multi-walled carbon nanotubes according to claim 1 or 2 or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method according to any one of claims 3 to 8 in preparing modified electrodes.

10. A modified electrode, It is characterized in that It includes an electrode and nickel-nitrogen doped multi-walled carbon nanotubes coated on the surface of the electrode; The nickel-nitrogen doped multi-walled carbon nanotubes are the nickel-nitrogen doped multi-walled carbon nanotubes according to claim 1 or 2 or the nickel-nitrogen doped multi-walled carbon nanotubes prepared by the preparation method according to any one of claims 3 to 8.

Citation Information

Patent Citations

  • Nickel-filled nitrogen-doped carbon nanotubes as well as preparation method and application thereof

    CN107570192A

  • Method for simultaneously determining dopamine and uric acid in copper-nickel nanometer material / multi-walled carbon nanotube composite membrane modified glassy carbon electrode

    CN108732233A

  • Doped multi-wall carbon nanotube, preparation methods therefor, and electrode material

    WO2022057114A1