Carbon nanotube suspension and preparation method and application thereof
By using Humilic acid and DNA as synergistic dispersants and combined with ultrasonic dispersion technology, the problem of poor stability of carbon nanotube suspension is solved, and efficient dispersion and suspension effects are achieved, which is suitable for adsorption of organic pollutants and heavy metals.
Patent Information
- Application Number
- CN202411215505.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-30
- Publication Date
- 2024-11-22
AI Technical Summary
Carbon nanotubes are prone to aggregation and settlement in water, making it difficult to prepare uniform and stable suspensions. The use effect of existing dispersion mechanisms such as Huminic acid is still poor.
Huminic acid and DNA are used as synergistic dispersants, and carbon nanotubes, Huminic acid and water are treated through ultrasonic dispersion technology to adjust the pH value and ultrasonic parameters to improve the stability and dispersion effect of the suspension.
It significantly improves the stability and dispersion effect of carbon nanotube suspension, enhances its suspension capability, and is suitable for adsorption of organic pollutants and heavy metals.
Smart Images

Figure CN118993043A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of carbon nanotubes, and in particular relates to a carbon nanotube suspension and a preparation method and application thereof. Background Art
[0002] Carbon-based nanomaterials refer to carbon materials with a size less than 100nm, and carbon nanotubes (CNTs) are a type of carbon-based nanomaterial. Due to their high hydrophobicity and van der Waals forces, carbon nanotubes are easily entangled with each other to form aggregates, which are very likely to aggregate and settle in the water phase, making it difficult to prepare a uniform and stable carbon nano suspension.
[0003] Regarding the dispersion problem of carbon nanotubes, the dispersion mechanisms that have been explored in the prior art mainly include electrostatic repulsion, steric hindrance effect, "zipper" mechanism and micellar dissolution mechanism, etc. For example, humic acid (HA) with a high aromatic content has an undeformable rigid structure, which can produce greater steric hindrance and has a stronger dispersion ability for carbon nanotubes. However, when using HA dispersant to disperse carbon nanotubes, the stability and dispersion effect of carbon nanotube suspensions are still poor. Summary of the invention
[0004] The purpose of the present invention is to provide a carbon nanotube suspension and a preparation method and application thereof. The preparation method provided by the present invention adopts humic acid and DNA double dispersants to synergistically disperse carbon nanotubes, and the carbon nanotube suspension has good stability and dispersion effect.
[0005] In order to achieve the above object, the present invention provides the following technical solutions:
[0006] The present invention provides a method for preparing a carbon nanotube suspension, comprising the following steps:
[0007] Humic acid, DNA, carbon nanotubes and water are ultrasonically dispersed and then allowed to stand to obtain a carbon nanotube suspension.
[0008] Preferably, the DNA comprises cDNA.
[0009] Preferably, the mass ratio of humic acid to DNA is 1:0.5-6.
[0010] Preferably, the carbon nanotubes include one or more of graphitized carbon nanotubes, carboxylated carbon nanotubes and hydroxylated carbon nanotubes;
[0011] The mass ratio of the carbon nanotubes to the DNA is 1:2-24.
[0012] Preferably, the ultrasonic power of the ultrasonic dispersion is 120-135W, the ultrasonic frequency is 0.17-0.5Hz, and the time is 15-45s;
[0013] The ultrasonic dispersion method is intermittent ultrasonic dispersion; the single ultrasonic time of the intermittent ultrasonic dispersion is 1 to 3 seconds, and the time interval between two adjacent ultrasonic times is 1 to 3 seconds.
[0014] Preferably, the standing temperature is 23-27° C. and the standing time is 20-28 hours.
[0015] Preferably, the ultrasonic dispersion comprises the following steps:
[0016] Dissolving humic acid in water to obtain a humic acid aqueous solution;
[0017] Dissolve DNA in water to obtain a DNA aqueous solution;
[0018] The carbon nanotubes, the humic acid aqueous solution and the DNA aqueous solution are ultrasonically dispersed.
[0019] Preferably, the pH values of the humic acid aqueous solution and the DNA aqueous solution are independently 6.8 to 7.2.
[0020] The present invention provides a carbon nanotube suspension prepared by the preparation method described in the above technical solution.
[0021] The present invention provides the use of the carbon nanotube suspension described in the above technical solution in the adsorption of organic pollutants or heavy metals.
[0022] The present invention ultrasonically disperses humic acid, DNA, carbon nanotubes and water and then stands to obtain a carbon nanotube suspension. Humic acid is a complex mixture of different acids containing carboxyl and phenolate groups, with a large molecular weight, strong aromaticity, and a rigid structure. It has a strong suspension ability for carbon nanotubes and can improve the stability of the carbon nanotube suspension; DNA has a small molecular weight and a chain-like flexible structure, which can effectively disperse carbon nanotubes. Humic acid and DNA are used to synergistically disperse carbon nanotubes, and the stability and dispersion effect of the obtained carbon nanotube suspension are excellent. The results of the embodiment show that graphitized carbon nanotubes, carboxylated carbon nanotubes and hydroxylated carbon nanotubes are most stably dispersed in a mixed solution in which the eDNA concentration is 40 mg / L, 40 mg / L and 10 mg / L respectively and the HA solution is 20 mg / L. BRIEF DESCRIPTION OF THE DRAWINGS
[0023] Figure 1 The graph is the absorbance and carbon nanotube particle size of the graphitized carbon nanotube suspension prepared in Example 1;
[0024] Figure 2The absorbance and carbon nanotube particle size diagram of the carboxylated carbon nanotube suspension prepared in Example 2;
[0025] Figure 3 This is a graph showing the absorbance of the hydroxylated carbon nanotube suspension prepared in Example 3 and the carbon nanotube particle size. DETAILED DESCRIPTION
[0026] The invention provides a method for preparing a carbon nanotube suspension, comprising the following steps: ultrasonically dispersing humic acid, DNA, carbon nanotubes and water and then standing the dispersion to obtain the carbon nanotube suspension.
[0027] In the present invention, unless otherwise specified, the reagents used are commercially available products well known to those skilled in the art.
[0028] In the present invention, the DNA preferably includes eDNA. In the present invention, the mass ratio of the humic acid to the DNA is preferably 1:0.5-6, more preferably 1:1-5, and most preferably 1:2-4.
[0029] In the present invention, the carbon nanotubes preferably include one or more of graphitized carbon nanotubes (G-CNTs), carboxylated carbon nanotubes (C-CNTs) and hydroxylated carbon nanotubes (H-CNTs). In the present invention, the mass ratio of the carbon nanotubes to DNA is preferably 1:2-24, more preferably 1:5-20, and most preferably 1:10-15.
[0030] In the present invention, the ultrasonic power of the ultrasonic dispersion is preferably 120-135W, more preferably 125-132W, and most preferably 128-130W; the ultrasonic frequency is preferably 0.17-0.5Hz, more preferably 0.2-0.3Hz, and most preferably 0.25-0.28Hz; the time is preferably 15-45s, more preferably 20-40s, and most preferably 30-35s. In the present invention, the ultrasonic dispersion method is preferably intermittent ultrasonic dispersion; the single ultrasonic time of the intermittent ultrasonic dispersion is preferably 1-3s, more preferably 1-2s; the time interval between two adjacent ultrasonic waves is preferably 1-3s, and more preferably 1-2s.
[0031] In the present invention, the ultrasonic dispersion preferably comprises the following steps:
[0032] Dissolve humic acid in water to obtain a humic acid aqueous solution; dissolve DNA in water to obtain a DNA aqueous solution; and ultrasonically disperse the carbon nanotubes, the humic acid aqueous solution and the DNA aqueous solution.
[0033] In the present invention, the concentration of the humic acid aqueous solution is preferably 15 to 35 mg / L, more preferably 18 to 30 mg / L, and most preferably 20 to 25 mg / L.
[0034] In the present invention, after dissolving humic acid in water, it is preferred to further include adjusting the pH value to >7, and then adjusting the pH value to neutral. The present invention does not specifically limit the type of alkali used to adjust the pH value to >7, and alkalis well known in the art can be used, such as sodium hydroxide and / or potassium hydroxide. The present invention does not specifically limit the type of acid used to adjust the pH value to neutral, and acids well known in the art can be used, such as hydrochloric acid. In the present invention, the pH value of the humic acid aqueous solution is preferably 6.8 to 7.2, more preferably 6.9 to 7.1, and most preferably 6.9 to 7.0. The present invention adopts an alkali dissolution and acid precipitation method, first adjusting the pH value to alkaline to dissolve the humic acid, and then adjusting the pH to neutral.
[0035] In the present invention, the concentration of the DNA aqueous solution is preferably 10 to 120 mg / L, more preferably 20 to 100 mg / L, and most preferably 40 to 60 mg / L; the pH value of the DNA aqueous solution is preferably 6.8 to 7.2, more preferably 6.9 to 7.1, and most preferably 6.9 to 7.0. In the present invention, the acid used to adjust the pH value of the DNA aqueous solution preferably includes hydrochloric acid.
[0036] In the present invention, the standing temperature is preferably 23-27°C, more preferably 24-26°C, and most preferably 24-25°C; the standing time is preferably 20-28h, more preferably 22-26h, and most preferably 24-25h; during the standing process, the carbon nanotubes are preferably in a suspended state.
[0037] The present invention provides a carbon nanotube suspension prepared by the preparation method described in the above technical solution. In the carbon nanotube suspension provided by the present invention, DNA can increase the dispersion amount of carbon nanotubes, and humic acid can improve the stability of the carbon nanotube suspension. The two are used as synergistic dispersants to enhance the suspension ability of carbon nanotubes, and the obtained carbon nanotube suspension has good stability and dispersion effect.
[0038] The present invention provides the use of the carbon nanotube suspension described in the above technical solution in organic pollutant adsorption or heavy metal adsorption. The carbon nanotube suspension provided by the present invention has good stability and dispersion effect, and when used in organic pollutant adsorption or heavy metal adsorption, it improves the adsorption effect and removal rate of heavy metals and organic pollutants.
[0039] In order to further illustrate the present invention, a carbon nanotube suspension and a preparation method thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.
[0040] In all the embodiments of the present invention, humic acid is obtained by extracting the soil from Heilongjiang Province (127.85° east, 42.8° north latitude) after natural air drying using an alkali-acid precipitation method (specifically, the humic acid is dissolved with an alkali and then adjusted back to neutral with an acid); eDNA is herring sperm DNA (hsDNA) purchased from Sigma-Aldrich; carbon nanotubes were purchased from Chengdu Zhongke Times Nano Co., Ltd.; and the device used for ultrasonic dispersion is a cell disruptor.
[0041] Example 1
[0042] Prepare eDNA aqueous solution with a series of concentrations and 20 mg / L humic acid aqueous solution in brown glass bottles, and adjust the pH value of the eDNA aqueous solution and humic acid aqueous solution to 7±0.2 with hydrochloric acid. The concentrations of the eDNA aqueous solution are 0 mg / L, 5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L, 25 mg / L, 30 mg / L, 40 mg / L and 60 mg / L.
[0043] Take 10 mL of the prepared humic acid aqueous solution into a 20 mL brown glass bottle, add 10 mL of the above eDNA aqueous solution to obtain a mixed dispersion;
[0044] 5 mg of graphitized carbon nanotubes were added to the mixed dispersion, and after ultrasonic dispersion for 30 seconds, the mixture was allowed to stand at 25° C. for 24 hours to obtain a graphitized carbon nanotube suspension, wherein the ultrasonic dispersion power was 127.5 W, the frequency was 0.25 Hz, the single ultrasonic time was 2 seconds, and the time interval between two ultrasonic times was 2 seconds.
[0045] Figure 1 The graph of the absorbance of the graphitized carbon nanotube suspension prepared in Example 1 and the carbon nanotube particle size is shown in FIG. Figure 1 It can be seen that with the gradual increase of eDNA concentration, the absorbance of the graphitized carbon nanotube suspension increased twice to different degrees when the eDNA concentration increased to 10 mg / L and 25 mg / L. When the DNA concentration increased to 40 mg / L, the absorbance decreased slightly, and the particle size first increased slightly and then decreased, and then remained stable. When the eDNA concentration increased to 40 mg / L, it decreased significantly and then increased slightly. When the eDNA concentration was 40 mg / L, the graphitized carbon nanotube suspension had the highest absorbance, the smallest particle size, and the graphitized carbon nanotube suspension was the most stable.
[0046] Example 2
[0047] The carboxylated carbon nanotube suspension was prepared by the preparation method provided in Example 1, which differs from Example 1 only in that the carbon nanotubes are carboxylated carbon nanotubes.
[0048] Figure 2The absorbance of the carboxylated carbon nanotube suspension prepared in Example 2 and the carbon nanotube particle size diagram are shown in FIG. Figure 2 It can be seen that as the eDNA concentration gradually increases, the absorbance of the carboxylated carbon nanotube suspension first increases significantly, and then fluctuates between 1.02 and 1.28, and its particle size first decreases, and then remains basically stable; when the eDNA concentration is 40 mg / L, the absorbance of the carboxylated carbon nanotube suspension is the highest, the particle size is smaller, and the carboxylated carbon nanotube suspension is the most stable.
[0049] Example 3
[0050] The hydroxylated carbon nanotube suspension was prepared by the preparation method provided in Example 1, which differs from Example 1 only in that the carbon nanotubes are hydroxylated carbon nanotubes.
[0051] Figure 3 The absorbance and carbon nanotube particle size of the hydroxylated carbon nanotube suspension prepared in Example 3 are shown in FIG. Figure 3 It can be seen that as the eDNA concentration gradually increases, the absorbance of the hydroxylated carbon nanotube suspension first increases significantly, and then fluctuates between 0.55 and 0.65, and its particle size first decreases and then remains unchanged; when the eDNA concentration is 10 mg / L, the hydroxylated carbon nanotube suspension has the highest absorbance, the smallest particle size, and the hydroxylated carbon nanotube suspension is the most stable.
[0052] Comparative Example 1
[0053] Prepare eDNA aqueous solutions of a series of concentrations in brown glass bottles, and adjust the pH value of the eDNA aqueous solution to 7±0.2 with hydrochloric acid. The concentrations of the eDNA aqueous solution are 5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L, 25 mg / L, 30 mg / L, 40 mg / L and 60 mg / L, respectively;
[0054] Take 10 mL of the prepared eDNA aqueous solution, add 5 mg of graphitized carbon nanotubes, and after ultrasonic dispersion for 30 seconds, stand at 25°C for 24 hours to obtain a graphitized carbon nanotube suspension, wherein the ultrasonic dispersion power is 127.5 W, the frequency is 0.25 Hz, the single ultrasonic time is 2 seconds, and the time interval between two ultrasonic times is 2 seconds.
[0055] Comparative Example 2
[0056] The carboxylated carbon nanotube suspension was prepared by the preparation method provided in Comparative Example 1, and the only difference from Comparative Example 1 is that the carbon nanotubes are carboxylated carbon nanotubes.
[0057] Comparative Example 3
[0058] The hydroxylated carbon nanotube suspension was prepared by the preparation method provided in Comparative Example 1, and the only difference from Comparative Example 1 is that the carbon nanotubes are hydroxylated carbon nanotubes.
[0059] The absorbance and particle size results of the carbon nanotube suspensions prepared in Comparative Examples 1 to 3 (graphitized carbon nanotube suspension, carboxylated carbon nanotube suspension and hydroxylated carbon nanotube suspension, respectively) at 800 nm are shown in Table 1.
[0060] Table 1 Absorbance and particle size of carbon nanotube suspensions prepared in Comparative Examples 1 to 3 at 800 nm
[0061]
[0062] As can be seen from Table 1, with the increase of eDNA concentration, the absorbance of the carbon nanotube suspension at 800nm shows an overall upward trend, while the particle size shows no obvious change or increase, indicating that with the increase of eDNA concentration, the dispersion amount of the carbon nanotube suspension also increases, but the stability does not increase significantly, and even decreases.
[0063] Comparative Example 4
[0064] A series of humic acid aqueous solutions were prepared in brown glass bottles, and the pH value of the humic acid aqueous solution was adjusted to 7±0.2 with hydrochloric acid. The concentrations of the humic acid aqueous solution were 5 mg / L, 10 mg / L, 15 mg / L, 20 mg / L, 25 mg / L, 30 mg / L, 40 mg / L and 60 mg / L, respectively;
[0065] 10 mL of the prepared humic acid aqueous solution was taken, 5 mg of graphitized carbon nanotubes were added, and after ultrasonic dispersion for 30 seconds, the mixture was allowed to stand at 25° C. for 24 hours to obtain a graphitized carbon nanotube suspension.
[0066] Comparative Example 5
[0067] The carboxylated carbon nanotube suspension was prepared by the preparation method provided in Comparative Example 4, which differs from Comparative Example 4 only in that the carbon nanotubes are carboxylated carbon nanotubes.
[0068] Comparative Example 6
[0069] The hydroxylated carbon nanotube suspension was prepared by the preparation method provided in Comparative Example 4, which differs from Comparative Example 4 only in that the carbon nanotubes are hydroxylated carbon nanotubes.
[0070] The absorbance and particle size results of the carbon nanotube suspensions prepared in Comparative Examples 4 to 6 (graphitized carbon nanotube suspension, carboxylated carbon nanotube suspension and hydroxylated carbon nanotube suspension, respectively) at 800 nm are shown in Table 2.
[0071] Table 2 Absorbance and particle size of carbon nanotube suspensions prepared in Comparative Examples 4 to 6 at 800 nm
[0072]
[0073] In the carbon nanotube suspensions prepared in Comparative Examples 4 to 6, as the concentration of humic acid increases, the absorbance of the carbon nanotube suspension at 800 nm increases and the particle size decreases, indicating that humic acid can increase the dispersion of carbon nanotubes and significantly improve the stability of the graphitized carbon nanotube suspension.
[0074] In summary, eDNA can significantly increase the dispersion amount of carbon nanotubes, while humic acid can significantly improve the stability of carbon nanotube suspensions. The use of eDNA and humic acid as synergistic dispersants can significantly enhance the suspension ability of carbon nanotubes, and the prepared carbon nanotube suspension has good stability and dispersibility.
[0075] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.
Claims
1. A method for preparing a carbon nanotube suspension, It is characterized in that The following steps are involved: Humic acid, DNA, carbon nanotubes and water are ultrasonically dispersed and then allowed to stand to obtain a carbon nanotube suspension.
2. The preparation method according to claim 1, It is characterized in that The DNA includes cDNA.
3. The preparation method according to claim 1 or 2, It is characterized in that The mass ratio of the humic acid to the DNA is 1:0.5-6.
4. The preparation method according to claim 1, It is characterized in that The carbon nanotubes include one or more of graphitized carbon nanotubes, carboxylated carbon nanotubes and hydroxylated carbon nanotubes; The mass ratio of the carbon nanotubes to the DNA is 1:2-24.
5. The preparation method according to claim 1, It is characterized in that The ultrasonic power of the ultrasonic dispersion is 120-135W, the ultrasonic frequency is 0.17-0.5Hz, and the time is 15-45s; The ultrasonic dispersion method is intermittent ultrasonic dispersion; the single ultrasonic time of the intermittent ultrasonic dispersion is 1 to 3 seconds, and the time interval between two adjacent ultrasonic times is 1 to 3 seconds.
6. The preparation method according to claim 1, It is characterized in that The standing temperature is 23-27° C. and the standing time is 20-28 hours.
7. The preparation method according to claim 1 or 5, It is characterized in that The ultrasonic dispersion comprises the following steps: Dissolving humic acid in water to obtain a humic acid aqueous solution; Dissolve DNA in water to obtain a DNA aqueous solution; The carbon nanotubes, the humic acid aqueous solution and the DNA aqueous solution are ultrasonically dispersed.
8. The preparation method according to claim 7, It is characterized in that The pH values of the humic acid aqueous solution and the DNA aqueous solution are independently 6.8-7.
2.
9. The carbon nanotube suspension obtained by the preparation method according to any one of claims 1 to 8.
10. Use of the carbon nanotube suspension according to claim 9 in the adsorption of organic pollutants or heavy metals.
Citation Information
Patent Citations
Method for preparing suspension liquid of steady Nano carbon tube by using tannic acid
CN101049925A
CNT (Carbon Nano Tube) coating material, preparation method thereof and optical fiber with coating
CN106242321A
Preparation method of water-based carbon hybrid material
CN110128784A
Modified multi-walled carbon nanotube, low-pressure membrane thereof, and preparation methods and applications of modified multi-walled carbon nanotube and low-pressure membrane
CN113104839A
Method for preparing carbon nanotube solution
CN116803902A