Preparation method of rare earth silicate

Through the mixed reaction and calcination of rare earth salt solution, alkaline solution and SiO2, the problems of pollution, time-consuming and labor-intensive and complex processes in the production of existing rare earth silicates are solved, and low-cost and low-impact rare earth silicates are achieved. Preparation, suitable for industrial production and preparation of lanthanum silicate powder with various structures.

CN118993094APending Publication Date: 2024-11-22BAOTOU RESEARCH INSTITUTE OF RARE EARTHS
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411112688.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing industrial large-scale production methods of rare earth silicates have problems such as ball mill pollution, time-consuming and labor-intensive, high cost and complex processes. The traditional high-temperature solid-phase firing and discharge plasma sintering process conditions are harsh, and the sol-gel method is inefficient. Not suitable for mass production.

Method used

The rare earth salt solution is mixed with alkaline solution and SiO2 to obtain the precursor and calcinate it to prepare rare earth silicate, avoiding discharge plasma technology and organic solvents. The process is simple and the cost is low, and it is suitable for lanthanum silicate of various structures. Powder preparation.

Benefits of technology

It realizes the low-cost, low-impact, simple and easy-to-operate preparation of rare earth silicates. It is suitable for industrial production, and the prepared sample is uniform in particle size, which is suitable for lanthanum silicate powders of various structures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993094A_ABST
    Figure CN118993094A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of rare earth silicate preparation, in particular to a preparation method of rare earth silicate. The preparation method of the rare earth silicate comprises the following steps: mixing and reacting a rare earth salt solution, an alkaline solution and SiO2 to obtain a precursor; and calcining the precursor to obtain the rare earth silicate. The preparation method is simple in process and easy to operate, and processes such as a discharge plasma technology with relatively harsh production conditions do not need to be used; no organic solvent is used, pollution is small, and industrialization is easy to achieve. Compared with a traditional high-temperature solid-phase method, the sample prepared by the method contains fewer impurities. The preparation method disclosed by the invention is low in cost, time-saving and energy-saving in process, easy to operate, simpler and more direct, and suitable for preparing lanthanum silicate powder with various different structures. The rare earth silicate prepared by the invention has a particle size D50 of 8-15 [mu] m, is easy to filter, and can be used in a thermal ring barrier coating material, a ceramic material or a refractory material.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of rare earth silicate preparation, in particular to a method for preparing rare earth silicate. Background Art

[0002] For a series of rare earth silicate compounds such as lanthanum orthosilicate, lanthanum disilicate, and apatite-type lanthanum silicate, the industrial large-scale production method is usually the traditional ball milling followed by high-temperature solid-phase firing, but ball milling can cause sample contamination, time-consuming and labor-intensive problems. Other preparation methods such as sol-gel method, combustion method, and organic precipitation method also have their own advantages and disadvantages, and have problems such as high cost, complicated process, and not conducive to large-scale production.

[0003] The invention patent with publication number CN117024129A discloses a method for preparing chromium-doped lanthanum disilicate ceramics, using LaCrO 3 and SiO 2 Powder, using spark plasma sintering technology at 1300 ~ 1500 ℃ directly prepared chromium doped La 2 Si 2 O 7 Ceramics. The invention utilizes LaCrO 3 With SiO 2 The powder is prepared into chromium-doped lanthanum disilicate ceramic blocks by discharge plasma technology, but the production process conditions using discharge plasma technology are relatively harsh.

[0004] The invention patent with publication number CN112029502A discloses a luminescent powder material of lanthanum silicate with apatite structure and its preparation method and application. Specifically, a coprecipitation method using tetraethyl orthosilicate as a raw material is used to prepare a luminescent powder material of lanthanum silicate with apatite structure. This method can successfully prepare a high-performance luminescent material without impurities. Among them, with lanthanum silicate as a matrix, the silicate luminescent powder has excellent thermal stability and chemical stability and low cost; with europium ions Eu 3+ As an activator, a luminescent powder material capable of emitting red light can be prepared. The invention also prepares apatite-structured lanthanum silicate without impurities, but requires ethyl orthosilicate as a raw material, which is costly and has a high risk factor.

[0005] The invention patent with publication number CN109264729A discloses a device and method for preparing lanthanum silicate nanopowder, which belongs to the field of lanthanum silicate nanopowder preparation. Lanthanum silicate nanopowder is prepared by using a sol-gel method, but the sol-gel method has high cost, difficult process control, low efficiency, and is not suitable for large-scale production.

[0006] The invention patent with publication number CN108264050A provides a method for preparing apatite-type lanthanum silicate, which is prepared by a precipitation reaction method from lanthanum salts and silicates that are easily soluble in water. The silicate ions are precipitated in the form of lanthanum silicate by utilizing the preferential reaction characteristics of lanthanum ions with silicate ions. The excess lanthanum ions react with alkaline solution to generate La(OH) 3 Precipitation, La(OH) 3 The invention requires that the soluble silicate and lanthanum ions are precipitated and then reacted with La(OH) 3 The co-precipitation and then calcination at high temperature is a complex process and difficult to control. Summary of the invention

[0007] In view of this, the present invention provides a method for preparing rare earth silicate.

[0008] To achieve the above object, the present invention provides the following solutions:

[0009] The present invention provides a method for preparing rare earth silicate, comprising the following steps:

[0010] Rare earth salt solution, alkaline solution and SiO 2 Mixing reaction to obtain a precursor;

[0011] The precursor is calcined to obtain the rare earth silicate.

[0012] In some embodiments of the present invention, the rare earth salt in the rare earth salt solution is at least one of rare earth chloride, rare earth nitrate, rare earth sulfate and rare earth acetate.

[0013] In some embodiments of the present invention, the alkaline solution is at least one of ammonium bicarbonate solution, ammonia water, ammonium carbonate solution, sodium bicarbonate solution and sodium carbonate solution, and the alkaline solution contains CO 3 2- .

[0014] In some embodiments of the present invention, the alkaline solution contains CO 3 2- The molar ratio to OH- is 1:(0~1).

[0015] In some embodiments of the present invention, the alkaline solution is CO 3 2- Timing, CO 3 2- The molar ratio of the rare earth ions in the rare earth salt solution is 1.5 to 1.8 (in terms of REO); the alkaline solution is HCO 3 - Timing, HCO 3 -The molar ratio to rare earth ions is 3 to 3.6.

[0016] In some embodiments of the present invention, the rare earth ions (in terms of REO) in the rare earth salt solution and the SiO 2 The molar ratio is (1~2):1.

[0017] In some embodiments of the present invention, the temperature of the mixing reaction is 10-60°C.

[0018] In some embodiments of the present invention, the calcination temperature is 1100-1500° C. and the calcination time is 2-7 hours.

[0019] In some embodiments of the present invention, the rare earth silicate is one or more of orthosilicic acid, disilicate, and apatite-type silicate.

[0020] The present invention discloses the following technical effects:

[0021] The preparation process of the present invention is simple and easy to operate, and does not require the use of processes with harsh production conditions such as discharge plasma technology; no organic solvent is used, the pollution is small, and it is easy to achieve industrialization. Compared with the traditional high-temperature solid phase method, the sample prepared by the present invention contains less impurities.

[0022] The preparation method of the invention has low cost, saves time and energy, is easy to operate, is simpler and more direct, and is suitable for preparing lanthanum silicate powders with various structures.

[0023] The rare earth silicate prepared by the invention has a D50 of 8-15 μm, is uniform in size and is easy to filter. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0025] Figure 1 The present invention is a process flow chart for preparing rare earth silicate.

[0026] Figure 2 The rare earth silicate (La 2 SiO 5 )’s XRD spectrum.

[0027] Figure 3 This is a particle size distribution diagram of the rare earth silicate prepared in Examples 1-3 of the present invention. DETAILED DESCRIPTION

[0028] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0029] It should be understood that the terms described in the present invention are only for describing a particular embodiment and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. The intermediate value in any stated value or stated range, and each smaller range between any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0030] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0031] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to the skilled artisan. The present invention description and examples are exemplary only.

[0032] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0033] In the present invention, REO means rare earth oxide, and D50 means the particle size corresponding to the cumulative particle size distribution number of the sample reaching 50%.

[0034] The present invention provides a method for preparing rare earth silicate, comprising the following steps:

[0035] Rare earth salt solution, alkaline solution and SiO 2 Mixing reaction to obtain a precursor;

[0036] The precursor is calcined to obtain the rare earth silicate.

[0037] In some embodiments of the present invention, the rare earth salt in the rare earth salt solution is at least one of rare earth chloride, rare earth nitrate, rare earth sulfate and rare earth acetate.

[0038] In some embodiments of the present invention, the alkaline solution is at least one of ammonium bicarbonate solution, ammonia water, ammonium carbonate solution, sodium bicarbonate solution and sodium carbonate solution, and the alkaline solution contains CO 3 2- . Further preferably, the alkaline solution is an ammonium bicarbonate solution.

[0039] In some embodiments of the present invention, the alkaline solution is CO 3 2- Time, in REO, CO 3 2- The molar ratio of the rare earth ions in the rare earth salt solution is 1.5 to 1.8; the alkaline solution is HCO 3 - Timing, HCO 3 - The molar ratio to rare earth ions is 3 to 3.6.

[0040] When the alkaline solution also contains OH - When the CO 3 2- With the OH - The molar ratio is 1:(0~1).

[0041] When the alkaline solution contains only hydroxide (i.e. ammonia water), rare earth hydroxide will be generated, which will become a colloid and is not easy to precipitate, affecting the uniform dispersion of silicon dioxide particles and rare earth components in the aqueous phase, and is not conducive to obtaining a stable pure product. Therefore, when there is ammonia water in the alkaline solution, the present invention will choose to mix ammonia water with other alkaline solutions.

[0042] In some embodiments of the present invention, the rare earth ions in the rare earth salt solution are 2 The molar ratio is (1~2):1.

[0043] In the present invention, when the molar ratio of rare earth ions to silicon dioxide is 2, calculated as REO, orthosilicate rare earth can be obtained; when the molar ratio of rare earth ions to silicon dioxide is 1, disilicate rare earth can be obtained; when the ratio of rare earth ions to silicon dioxide is 1.556-1.667, apatite-type rare earth silicate can be obtained; when the molar ratio of rare earth ions to silicon dioxide is in other ranges, the product is a mixed phase of various crystalline rare earth silicates.

[0044] In some embodiments of the present invention, the SiO 2 D 50 The particle size is 1 to 5 μm and is required to be evenly distributed and concentrated.

[0045] SiO 2Too large or too small D50 particle size will affect the final product rare earth silicate. If it is too small, the nano-scale particles will agglomerate severely and will not be conducive to uniform dispersion in water. After precipitation, it will cause uneven local packaging. If it is too large, the SiO 2 The lanthanum carbonate inside and outside the particles is not in sufficient contact, resulting in uneven distribution. Impurity phases or direct precipitation and pyrolysis of rare earth raw materials in the final product will generate by-products.

[0046] In some embodiments of the present invention, the concentration of the alkaline solution is 0.6-2.8 mol / L.

[0047] In some embodiments of the present invention, the calcination temperature is 1100-1500°C and the time is 2-7 hours. More preferably, the calcination temperature is 1250°C.

[0048] In some embodiments of the present invention, the rare earth silicate is one or more of orthosilicic acid, disilicate, and apatite-type silicate. The chemical formula of the rare earth silicate is RE x Si y O z ; Wherein x=2, 9.33~10; y=1, 2, 6; z=5, 7, 26~27.

[0049] In some embodiments of the present invention, rare earth salt solution, alkaline solution and SiO 2 The following mixing methods can be used for the reaction:

[0050] The first mixing method: the target ratio of silicon dioxide and rare earth salt solution is mixed and slurried evenly as the base liquid, and the alkaline solution is added dropwise into the base liquid under heating and stirring conditions to a pH value of 6.7 to 7.6. The precursor obtained is a cross-shaped block of rare earth carbonate and silicon dioxide particles.

[0051] The second mixing method: the target ratio of silicon dioxide and alkaline solution are mixed and slurried evenly as the base liquid, and the rare earth salt solution is added dropwise into the base liquid under heating and stirring conditions to a pH value of 6.7 to 7.6, and the precursor obtained is a nano-sheet rare earth carbonate layer intercalated with silicon dioxide particles;

[0052] The third mixing method: Mix the target proportion of silicon dioxide with water to make a uniform slurry as the base liquid, and add the rare earth salt solution and the alkaline solution simultaneously under heating and stirring conditions to the reaction pH value of 6.7-7.6. The obtained precursor is a uniform cluster-like particle composed of nano-flake rare earth carbonate-wrapped silicon dioxide particles.

[0053] In the third mixing method, the silica particles are fully dispersed in the aqueous phase to provide conditions for the precipitation of lanthanum carbonate to wrap the silica particles; the amount of slurry mixing water used is 1 / 10 of the volume of the total reaction system (silicon dioxide, rare earth salt solution and alkaline solution).

[0054] More preferably, a third mixing method is adopted.

[0055] In the present invention, the condition that affects the synthesis of rare earth silicate (lanthanum silicate) is the mixing method. The morphology of lanthanum carbonate precursors prepared by different mixing methods is different, which makes the distribution state and uniformity of silicon dioxide and lanthanum carbonate precursor different. The third mixing method mixes the two more fully, and the conversion rate of preparing rare earth silicate is higher.

[0056] In some embodiments of the present invention, the conditions of the mixed reaction are as follows: heating temperature 10-60°C, preferably 40°C; stirring speed 250-400rpm, preferably 300rpm; reaction time 40-180min, preferably 60min; the pH value at the reaction end point is 6.7-7.6, preferably pH 7.0. After the reaction is completed, the steps of filtering, washing and drying are also included.

[0057] The process flow chart of the present invention for preparing rare earth silicate is as follows Figure 1 shown.

[0058] Unless otherwise specified, the raw materials used in the embodiments of the present invention can be obtained through commercial sources.

[0059] LaCl used in the embodiments of the present invention 3 The solution was prepared by mixing LaCl 3 Add to water and dissolve.

[0060] NH used in the embodiments of the present invention 4 HCO 3 The solution was made by 4 HCO 3 Add to water and dissolve.

[0061] The SiO used in the embodiments of the present invention 2 The average particle size of the particles was 2.5 μm.

[0062] Here is the test method:

[0063] X-ray diffraction: The particle size D was measured using an X-ray powder diffractometer (model: X Pert PRO) from PANalytical, the Netherlands. 50 : The test was carried out using Mastersizer 3000 laser particle size analyzer.

[0064] The concentration of the rare earth salt solution described in the embodiments of the present invention refers to the concentration of REO.

[0065] The present invention will be further described below by way of examples.

[0066] Example 1

[0067] Take 434.4mL of 150g / L LaCl 3 Solution, 12.0 g SiO 2 Particles, 500mL of 2.6mol / L NH 4 HCO 3 solution as raw material. 2 The particles were mixed with 1 / 10 of the total reaction system volume of water to form a uniform slurry as the base liquid. LaCl 3 Solution with NH 4 HCO 3 The solution was simultaneously added to the bottom liquid in parallel to form a precipitate until the pH value of the slurry was 7.0. The reaction time was controlled within 60 minutes. The obtained solid-liquid mixture was filtered, washed, and dried to obtain a precursor of lanthanum carbonate coating silica particles. The precursor was kept at 1250° C. for 3 hours, cooled and taken out to obtain lanthanum orthosilicate La 2 SiO 5 Powder material.

[0068] The La prepared in this example was analyzed by DX-27mini desktop diffractometer. 2 SiO 5 The powder material was tested and the results were as follows Figure 2 As shown by Figure 2 It can be seen that the pure phase La obtained in Example 1 2 SiO 5 The powder has no characteristic peaks of lanthanum oxide, silicon dioxide and other phases of lanthanum silicate in the XRD spectrum, which shows that the method of the present invention can be used to easily obtain pure phase La 2 SiO 5 Powder.

[0069] Example 2

[0070] Take 434.4mL of 150g / L LaCl 3 Solution, 24.0 g SiO 2 Particles, 500mL of 2.6mol / L NH 4 HCO 3 solution as raw material. 2The particles were mixed with 1 / 10 of the total reaction system volume of water to form a uniform slurry as the base liquid. LaCl 3 Solution with NH 4 HCO 3 The solution was simultaneously added to the bottom liquid in parallel to form a precipitate until the pH value of the slurry was 7.0. The reaction time was controlled within 60 minutes. The solid-liquid mixture was filtered, washed, and dried to obtain a precursor of lanthanum carbonate coating silica particles. The precursor was kept at 1250°C for 3 hours, cooled and taken out to obtain La 2 Si 2 O 7 Powder material.

[0071] Example 3

[0072] Take 434.4mL of 150g / L LaCl 3 Solution, 15.4 g SiO 2 Particles, 500mL of 2.6mol / L NH 4 HCO 3 solution as raw material. 2 The particles were mixed with 1 / 10 of the total reaction system volume of water to form a uniform slurry as the base liquid. LaCl 3 Solution with NH 4 HCO 3 The solution was simultaneously added to the bottom liquid in parallel to form a precipitate until the pH value of the slurry was 7.0. The reaction time was controlled within 120 min. The solid-liquid mixture was filtered, washed, and dried to obtain a precursor of lanthanum carbonate coating silica particles. The precursor was kept at 1200 ° C for 3 h, cooled and taken out to obtain La 9.33 Si 6 O 26 Powder material.

[0073] The particle size distribution of the rare earth silicate prepared in Examples 1-3 is as follows: Figure 3 As shown. Figure 3 It can be seen that the particle size of lanthanum silicate prepared by this method is relatively uniform, and the D50 size is less than 15 μm.

[0074] Comparative Example 1

[0075] Take 434.4mL of 150g / L LaCl 3 Solution, 11 g SiO 2 Particles, 500mL of 2.6mol / L NH 4 HCO 3 solution as raw material. 2The particles were mixed with 1 / 10 of the total reaction system volume of water to form a uniform slurry as the base liquid. LaCl 3 Solution with NH 4 HCO 3 The solution was simultaneously added to the bottom liquid in parallel to form a precipitate until the pH value of the slurry was 7.0. The reaction time was controlled within 60 minutes. The solid-liquid mixture was filtered, washed, and dried to obtain a precursor of lanthanum carbonate coating silica particles. The precursor was kept at 1250°C for 3 hours, cooled and taken out to obtain La 2 Si 2 O 7 ,La 9.33 Si 6 O 26 with La 2 O 3 Mixed crystal powder.

[0076] Comparative Example 2

[0077] Take 434.4mL of 150g / L LaCl 3 Solution, 26.7 g SiO 2 Particles, 500mL of 2.6mol / L NH 4 HCO 3 solution as raw material. 2 The particles were mixed with 1 / 10 of the total reaction system volume of water to form a uniform slurry as the base liquid. LaCl 3 Solution with NH 4 HCO 3 The solution was simultaneously added to the bottom liquid in parallel to form a precipitate until the pH value of the slurry was 7.0. The reaction time was controlled within 60 minutes. The solid-liquid mixture was filtered, washed, and dried to obtain a precursor of lanthanum carbonate coating silica particles. The precursor was kept at 1250°C for 3 hours, cooled and taken out to obtain La 2 Si 2 O 7 ,La 9.33 Si 6 O 26 With SiO 2 Mixed crystal powder.

[0078] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A method for preparing rare earth silicate, characterized in that: The following steps are involved: Mixing rare earth salt solution, alkaline solution and SiO2 to react and obtain a precursor; The precursor is calcined to obtain the rare earth silicate.

2. The method for preparing rare earth silicate according to claim 1, characterized in that: The rare earth salt in the rare earth salt solution is at least one of rare earth chloride, rare earth nitrate, rare earth sulfate and rare earth acetate.

3. The method for preparing rare earth silicate according to claim 1, characterized in that: The alkaline solution is at least one of ammonium bicarbonate solution, ammonia water, ammonium carbonate solution, sodium bicarbonate solution and sodium carbonate solution, and the alkaline solution contains CO3 2- .

4. The method for preparing rare earth silicate according to claim 1, characterized in that: The alkaline solution contains CO3 2- With OH - The molar ratio is 1:(0~1).

5. The method for preparing rare earth silicate according to claim 1, characterized in that: The alkaline solution is CO3 2- Timing, CO3 2- The molar ratio of the rare earth ions in the rare earth salt solution is 1.5 to 1.8; the alkaline solution is HCO3 - Timer, HCO3 - The molar ratio to rare earth ions is 3 to 3.

6.

6. The method for preparing rare earth silicate according to claim 1, characterized in that: Calculated in terms of REO, the molar ratio of the rare earth ions in the rare earth salt solution to the SiO2 is (1-2):

1.

7. The method for preparing rare earth silicate according to claim 1, characterized in that: The temperature of the mixed reaction is 10-60°C.

8. The method for preparing rare earth silicate according to claim 1, characterized in that: The calcination temperature is 1100-1500° C. and the calcination time is 2-7 hours.

9. The method for preparing rare earth silicate according to claim 1, characterized in that: The rare earth silicate is one or more of orthosilicic acid, disilicate and apatite type silicate.

Citation Information

Patent Citations

  • Preparation method of composite rare earth silicate powder

    CN106342076B

  • Carbon coating-coprecipitation preparation method of Yb2Si2O7 ultrafine powder

    CN112479724A

  • Process for obtaining a rare earth silicate glass composition and process for the production of said silicate

    EP0486352A1

  • Method for producing apatite-type rare earth silicate

    JP2023130940A

  • Spraying particles and manufacturing method thereof

    US20200190334A1