High-activity electrode, preparation method thereof and application of high-activity electrode in sewage treatment

By doping rare earth element Tb in titanium-based tin dioxide-antimal electrodes, a highly reactive titanium-based tin dioxide-antimal electrode was prepared, which solved the problems of low degradation efficiency and short life of existing electrodes, and achieved more efficient antibiotics Improved wastewater treatment and electrocatalytic performance.

CN118993254AActive Publication Date: 2024-11-22SHANDONG UNIV
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411237679.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-05
Publication Date
2024-11-22
Estimated Expiration
2044-09-05

AI Technical Summary

Technical Problem

The existing titanium-based tin dioxide-antimone electrode has low degradation efficiency and short service life when treating antibiotic wastewater, and the coating is brittle and easy to fall off, and its stability is insufficient.

Method used

By configuring the Sn source, Sb source and Tb source into a mixed solution, the Tb-Sn-Sb sol was obtained after ultrasonic treatment and static aging, uniformly applied to the surface of the electrode substrate, and heat treatment was performed at a specific temperature to prepare high Active titanium-based tin dioxide-antimal electrode improves its conductivity and electrocatalytic properties.

Benefits of technology

The electrode's electrocatalytic activity and service life are significantly improved, and can be reused three times or more without reducing the degradation rate, shortening the pollutant degradation time, reducing energy consumption, and improving the electrode's dense uniform coating and conductivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993254A_ABST
    Figure CN118993254A_ABST
Patent Text Reader

Abstract

The invention discloses a high-activity electrode, a preparation method thereof and application of the high-activity electrode in sewage treatment. The preparation method comprises the following steps: preparing a Sn source, an Sb source and a Tb source into a mixed solution, carrying out ultrasonic treatment, standing and aging to obtain Tb-Sn-Sb sol, uniformly coating the surface of an electrode substrate with the Tb-Sn-Sb sol, and carrying out heat treatment at a specific temperature to obtain the high-activity titanium-based tin dioxide-antimony electrode. It is found for the first time that the Ti / SnO2-Sb electrode is doped with the rare earth element Tb, the conductivity of the Ti / SnO2-Sb electrode can be greatly improved, and the treatment capacity of the Ti / SnO2-Sb electrode on waste water containing organic pollutants can be greatly improved. The removal rate of the Ti / SnO2-Sb-Tb electrode to the moxifloxacin reaches 84% or above, while the removal rate of the conventional Ti / SnO2-Sb electrode to the moxifloxacin is only 58.4%, and the removal rate of the Ti / SnO2-Sb-Ho electrode doped with other rare earth elements to the moxifloxacin is 74.1%. The invention further shows that the rare earth element Tb is doped in the Ti / SnO2-Sb electrode, so that the treatment capacity of the electrode on wastewater containing organic pollutants can be greatly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a highly active electrode, a preparation method thereof, and applications in sewage treatment, and specifically to a titanium-based tin dioxide-antimony electrode with higher electrode activity, stronger electrocatalytic performance, and longer life, a preparation method thereof, and applications in treating antibiotic-containing wastewater, belonging to the technical field of electrochemical water treatment. Background Art

[0002] Antibiotics are broad-spectrum drugs used to treat human and animal diseases and effectively inhibit microbial growth. However, the continued detection of antibiotic residues in water bodies has drawn global attention and created a range of environmental problems. Furthermore, antibiotic residues in the environment can negatively impact organisms, such as endocrine disruption and genotoxicity. Pharmaceutical wastewater requires treatment before discharge. Approximately 70% of these antibiotics are excreted from humans and animals into the environment in a stable state, resulting in high concentrations of antibiotics remaining in wastewater, soil, and sediment.

[0003] The current treatment technologies and methods for antibiotic wastewater mainly include adsorption, photodegradation, electrolysis, membrane separation, reduction, etc. Exploring efficient and economical antibiotic wastewater treatment technologies has important practical and theoretical significance. At present, electrochemical oxidation technology is mostly used for wastewater that is difficult to degrade because it has the characteristics of easy operation of equipment, no secondary pollution, and is considered to be an environmentally friendly method. Therefore, electrochemical treatment technology has good prospects in wastewater treatment methods. In electrochemical reactions, the role of electrodes is dominant. Finding high-performance electrode materials and exploring the influence of the selection of electrode materials on the electrocatalytic effect are particularly important in electrocatalytic reactions.

[0004] Electrochemical oxidation technology has the characteristics of high removal efficiency, simple operation process, low cost, and no secondary pollution. It has gradually become one of the most promising technologies in the field of water treatment. The electrode is the core component in the electrocatalytic oxidation technology that affects the conductivity efficiency, electron transfer rate, and the difficulty of generating activated reactants. The choice of electrode material will directly affect the quality of the electrocatalytic performance. Although precious metal electrocatalysts such as Pt and RuO2 have outstanding performance in the field of electrocatalysis, they are greatly restricted in application due to their high cost and scarcity. The DSA electrode is formed by coating the conventional electrode substrate. The Ti-SnO2 electrode is the most widely used electrode anode material in wastewater treatment. Rare earth element doped Ti / SnO2-Sb electrode can effectively change the surface morphology and lattice parameters of the metal oxide electrode, so that the oxygen evolution potential, electrocatalytic activity and service life of the electrode are improved to a certain extent;

[0005] The conventional titanium-based tin dioxide-antimony electrodes currently used have several drawbacks, including a brittle coating that easily peels off and insufficient stability during electrolysis. Therefore, it is necessary to modify the Ti / SnO2-Sb electrode by doping to further enhance its catalytic activity and stability.

[0006] Rare earth elements (RE), due to their unique unpaired 4f electrons, have unique potential for electrode doping to improve catalytic performance. Lanthanide rare earth compounds possess a rich energy level structure and unique ff electron transitions, resulting in long luminescence lifetimes, high luminescence efficiency, and large Stokes shifts. They are widely used in luminescence, electrocatalysis, and magnetism, and hold great promise for electrochemistry. Summary of the Invention

[0007] To address the shortcomings of existing technologies, the present invention provides a highly active electrode, a preparation method thereof, and its application in sewage treatment. The highly active electrode provided by the present invention can address the problems of low pollutant degradation efficiency and short electrode service life of conventional Ti / SnO2-Sb electrodes. It can also shorten pollutant degradation time and significantly reduce experimental energy consumption. The electrode can be reused three or more times without reducing the degradation rate. Furthermore, the surface coating of the highly active electrode prepared is denser and more uniform, significantly improving the electrode's electrocatalytic performance and electrical conductivity. Summary of the invention:

[0009] The present invention prepares a mixed solution of Sn, Sb, and Tb sources, ultrasonically treats the solution, and then allows it to age to obtain a Tb-Sn-Sb sol. The Tb-Sn-Sb sol is then uniformly coated on the surface of an electrode substrate. Heat treatment at a specific temperature produces a highly active titanium-based tin dioxide-antimony electrode. The resulting titanium-based tin dioxide-antimony electrode coating has a denser and more uniform surface, smaller grain size, improved electrical conductivity, better performance, and a longer lifespan. This electrode will be used to treat fluorine-containing antibiotic (moxifloxacin) wastewater. Detailed description of the invention:

[0011] A method for preparing a highly active titanium-based tin dioxide-antimony electrode comprises the following steps:

[0012] (1) adding Sn source, Sb source and Tb source to an organic solvent to prepare a mixed solution, wherein the molar concentration ratio of the Sn source, Sb source and Tb source in the mixed solution is Sn:Sb:Tb=100:10:(0.1-2); then ultrasonicating the mixed solution at 50-150 Hz for 10-20 minutes, and allowing it to stand for 1-2 hours to obtain a Tb-Sn-Sb sol;

[0013] (2) completely immersing the pretreated electrode substrate in the Tb-Sn-Sb sol obtained in step (1), taking it out and evenly smearing the Tb-Sn-Sb sol on the surface of the electrode substrate with a soft brush, then drying the coated electrode substrate at 100-130°C for 10-20 minutes, and then heat treating it at 450-600°C for 10-30 minutes, taking it out and cooling it to room temperature, washing the surface with deionized water, and drying it;

[0014] (3) Repeat the complete immersion and coating of step (2) 5 to 9 times, dry the electrode substrate after the last complete immersion and coating at 100 to 130° C. for 10 to 20 minutes, and then calcine at 550 to 700° C. for 1 to 2 hours. After taking it out, cool it to room temperature, clean the surface with deionized water and dry it to obtain a highly active titanium-based tin dioxide-antimony electrode.

[0015] According to the preferred embodiment of the present invention, in step (1), the Sn source is crystalline tin tetrachloride, the Sb source is antimony trichloride, and the Tb source is terbium nitrate.

[0016] According to the present invention, preferably, in step (1), the organic solvent is a citric acid ethylene glycol solution, and the total molar number of the Sn source and the Sb source in the mixed solution is: citric acid: ethylene glycol = 1: (2 to 5): (8 to 12).

[0017] Further preferably, in step (1), the organic solvent is an ethylene glycol solution of citric acid, and the total molar number of the Sn source and the Sb source in the mixed solution is: citric acid:ethylene glycol = 1:3:10.

[0018] Preferably, according to the present invention, in step (1), the ion molar concentration ratio of the Sn source, Sb source and Tb source is Sn:Sb:Tb=100:10:1.5.

[0019] According to the preferred embodiment of the present invention, in step (2), the electrode substrate is a titanium mesh, and the pretreatment method thereof is: polishing, alkali washing, acid washing in sequence, ultrasonic cleaning at 100 Hz for 10 minutes, and then cleaning with deionized water, placing it in an oven to dry, and the pretreated electrode substrate is stored in anhydrous ethanol.

[0020] According to the preferred embodiment of the present invention, in step (2), the coated electrode substrate is placed in an electric blast drying oven and dried at 130° C. for 20 minutes, and then placed in a muffle furnace and heat treated at 500° C. for 20 minutes.

[0021] According to the preferred embodiment of the present invention, in step (3), the number of repeated complete immersion and coating is 6 times. After the last coating is completed, the electrode substrate is placed in an electric blast drying oven and dried at 130°C for 20 minutes, and then placed in a muffle furnace and baked at 600°C for 2 hours, and then taken out and cooled to room temperature.

[0022] The present invention provides a high-activity titanium-based tin dioxide-antimony electrode prepared by the above method.

[0023] The present invention also provides the use of a high-activity titanium-based tin dioxide-antimony electrode in treating wastewater containing organic pollutants.

[0024] Preferably according to the present invention, the organic pollutant is a fluoroquinolone antibiotic.

[0025] Beneficial effects:

[0026] 1. The present invention discovered for the first time that doping the rare earth element Tb into the Ti / SnO2-Sb electrode can significantly improve the conductivity of the Ti / SnO2-Sb electrode and its ability to treat wastewater containing organic pollutants.

[0027] 2. The highly active titanium-based tin dioxide-antimony electrode of the present invention has a strong ability to degrade organic pollutants. Experiments using a solution of moxifloxacin (MOX) raw material to simulate fluorine-containing antibiotic wastewater showed that the Ti / SnO2-Sb-Tb electrode of the present invention achieved a moxifloxacin (MOX) removal rate of over 84%, while a conventional Ti / SnO2-Sb electrode achieved a moxifloxacin (MOX) removal rate of only 58.4%. A Ti / SnO2-Sb-Ho electrode doped with other rare earth elements achieved a moxifloxacin (MOX) removal rate of 74.1%. This demonstrates that doping the Ti / SnO2-Sb electrode with the rare earth element Tb significantly improves the electrode's ability to treat wastewater containing organic pollutants. Furthermore, the highly active titanium-based tin dioxide-antimony electrode of the present invention can also be used to treat other toxic and hazardous, difficult-to-degrade organic pollutants in aquatic environments.

[0028] 3. The present invention uses a Tb-Sn-Sb sol to coat the surface of the electrode substrate, combining a brushing method with heat treatment at a specific temperature to produce a highly active titanium-based tin dioxide-antimony electrode. This highly active titanium-based tin dioxide-antimony electrode has a denser and more uniform coating surface, higher surface crystallinity, and smaller grain size, increasing the electrode's specific surface area and thus increasing contact between the electrode and the target pollutant. This improves the electrode's electrical conductivity, performance, and electrocatalytic activity.

[0029] 4. The present invention provides a method for preparing a highly active titanium-based tin dioxide-antimony electrode. This method combines a brushing method with heat treatment at a specific temperature. It is simple to operate, uses Tb as the doping raw material, and has low material costs. Furthermore, this method can degrade difficult-to-degrade organic matter at room temperature and pressure. The reaction conditions are mild, the reaction apparatus is simple, and the reaction time is significantly shortened, significantly reducing energy consumption and facilitating scale-up. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 These are photographs of the surfaces of the highly active titanium-based tin dioxide-antimony electrode of Example 1 and the electrode of Comparative Example 1, taken at magnifications of 1000 times and 200 times under scanning electron microscopes;

[0031] In the figure, a and c are the Ti / SnO2-Sb electrodes of Comparative Example 1; b and d are the high-activity rare earth Tb-modified titanium-based tin dioxide-antimony electrodes of Example 1.

[0032] Figure 2 This is a comparison picture of the X-ray diffraction (XRD) analysis patterns of the high-activity titanium-based tin dioxide-antimony electrode of Example 1 and the electrode of Comparative Example 1.

[0033] Figure 3 This is a graph showing the removal rate during the electrochemical degradation of moxifloxacin (MOX) solution simulating the degradation of fluorine-containing antibiotic wastewater by the high-activity titanium-based tin dioxide-antimony electrode of Example 1, the Ti / SnO2-Sb electrode of Comparative Example 1, and the Ti / SnO2-Sb-Ho electrode of Comparative Example 2. DETAILED DESCRIPTION

[0034] The present invention will be described in detail below with reference to the accompanying drawings to make its objectives, advantages and technical solutions clearer, but they should not be understood as limiting the present invention.

[0035] Example 1

[0036] A method for preparing a highly active Ti / SnO2-Sb-Tb electrode comprises the following steps:

[0037] (1) Pretreatment of electrode substrate

[0038] ①. Selection of electrode substrate: The anode material is a 30mm×40mm×1mm titanium mesh, and the cathode material is a 30mm×40mm×1mm titanium plate;

[0039] ② Polishing the electrode substrate: First, use 180-mesh sandpaper to polish the surface of the titanium mesh and titanium plate over a large area, then continue polishing the titanium mesh and titanium plate with 300-mesh sandpaper to remove the oxides on their surfaces until the surface of the titanium substrate presents a silvery-white metallic luster. Finally, place the polished titanium mesh and titanium plate in deionized water and clean them in 100Hz ultrasonic waves for 10 minutes to clean the oxides that have fallen into the gaps of the titanium mesh and the corners of the titanium plate. Use an oven or a hair dryer to dry the water on the cleaned electrode surface and set aside.

[0040] ③. Preprocessing:

[0041] a. Alkali washing: Place the polished and cleaned titanium mesh and titanium plate in a 5% sodium carbonate solution. After heating to boiling, alkali wash the titanium mesh and titanium plate for 1 hour to remove the oil stains on the electrode surface. After the alkali washing cools down, clean the electrode surface with deionized water.

[0042] b. Pickling: Then place the alkali-washed titanium mesh and titanium plate in a 10% mass fraction oxalic acid solution, wait for it to boil, and pickle for 2 to 3 hours to remove the residual oxides on the surface of the titanium mesh and titanium plate. During the pickling and etching process of the titanium mesh and titanium plate, it can be observed that the oxalic acid solution gradually changes from transparent to yellow and finally to black. This is because the oxalic acid solution reacts with the oxides on the surface of the titanium mesh and titanium plate during the heating process. The titanium mesh and titanium plate after pickling appear yellow-brown. The titanium plate and titanium mesh after pickling are ultrasonically cleaned to remove the residual oxalic acid solution on the surface;

[0043] c. Secondary alkali washing and acid washing: The cleaned titanium mesh and titanium plate are subjected to secondary alkali washing and acid washing again, and the pickled titanium mesh and titanium plate are placed in a 5% by mass sodium carbonate solution for secondary alkali washing to remove the oxalic acid solution remaining on the surface of the electrode substrate. After the surface of the electrode substrate is cleaned with deionized water, it is placed in an oxalic acid solution to clean the residual sodium carbonate solution on the surface again; the surface of the electrode substrate after the secondary acid and alkali washing is in a pockmarked state; the surface of the titanium mesh and titanium plate treated with the secondary alkali washing and acid washing is cleaned with deionized water and ultrasonicated for 10 minutes to remove impurities remaining on the surface; finally, the cleaned titanium mesh and titanium plate are placed in an 80°C oven to dry the surface moisture to obtain a surface-dried electrode substrate, which is then placed in anhydrous ethanol for storage.

[0044] (2) Preparation of Tb-Sn-Sb sol

[0045] Ethylene glycol is placed in a water bath and heated to 65°C at a constant temperature, and citric acid is added and stirred until completely dissolved to obtain an ethylene glycol solution of citric acid; then the temperature is raised to 90°C, and tin tetrachloride (SnCl4), antimony trichloride SbCl3 and terbium nitrate (Tb·3NO3·6H2O) are added to the organic solvent in a molar ratio of Sn:Sb:Tb=100:10:1.5, and the mixture is heated and stirred in a 90°C constant temperature water bath until dissolved to obtain a yellow-green mixed solution. After cooling, the mixed solution is ultrasonicated at 100 Hz for 15 minutes and allowed to stand for 1.5 hours to obtain a Tb-Sn-Sb sol;

[0046] The total molar number of the Sn source and the Sb source in the mixed solution is 1:3:10 in terms of citric acid and ethylene glycol.

[0047] (3) Preparation of highly active Ti / SnO2-Sb-Tb electrodes

[0048] The pretreated titanium mesh was rinsed with deionized water and dried in an oven at 100°C for 15 minutes to obtain a dried titanium mesh substrate; the titanium mesh substrate was then completely immersed in the Tb-Sn-Sb sol, and after being taken out, the Tb-Sn-Sb sol was fully contacted and brushed with a soft brush on the surface of the titanium mesh substrate so that the coating liquid evenly covered the surface of the titanium mesh substrate; the coated titanium mesh substrate was then placed in a 130°C electric blast drying oven for 20 minutes, and then placed in a muffle furnace for heat treatment at 500°C for 20 minutes. After being taken out, it was cooled to room temperature, the surface was washed with deionized water, and dried;

[0049] Then, the titanium mesh substrate was completely immersed and coated again, and repeated 6 times (a total of 7 complete immersion and coating operations). After the last coating, the titanium mesh substrate was placed in an electric blast drying oven and dried at 130°C for 20 minutes. It was then placed in a muffle furnace and calcined at 600°C for 2 hours. After being taken out, it was cooled to room temperature, the surface was cleaned with deionized water, and it was placed in an oven at 80°C and dried for 15 minutes until completely dry to obtain a highly active Ti / SnO2-Sb-Tb electrode.

[0050] Example 2

[0051] A method for preparing a highly active Ti / SnO2-Sb-Tb electrode, the specific steps of which are the same as those of Example 1, except that in step (2), the ion molar concentration ratio of tin tetrachloride (SnCl4), antimony trichloride SbCl3 and terbium nitrate (Tb·3NO3·6H2O) is Sn:Sb:Tb=100:10:2.

[0052] Example 3

[0053] A method for preparing a highly active Ti / SnO2-Sb-Tb electrode, wherein the specific steps are the same as those of Example 1, except that in step (2) and step (3), the electrode coating is applied a total of 10 times.

[0054] Example 4

[0055] A method for preparing a high-activity Ti / SnO2-Sb-Tb electrode, the specific steps are the same as those in Example 1, except that in step (2) and step (3), the titanium mesh substrate after the last complete immersion and coating is placed in a box-type resistance furnace and calcined at 700°C for 2 hours.

[0056] Comparative Example 1

[0057] A method for preparing a Ti / SnO2-Sb electrode comprises the following steps:

[0058] (1) The pretreatment of the electrode substrate was carried out according to the method of Example 1;

[0059] (2) placing ethylene glycol in a water bath and heating it to 65°C, then adding citric acid and stirring until completely dissolved to obtain a citric acid ethylene glycol solution; then heating it to 90°C, adding tin tetrachloride (SnCl4) and antimony trichloride SbCl3 to the organic solvent in a molar ratio of Sn:Sb=10:1, heating and stirring in a 90°C constant temperature water bath until dissolved to obtain a mixed solution, and after cooling, ultrasonicating the mixed solution at 100 Hz for 15 minutes to obtain a Sn-Sb sol; wherein the total molar number of the Sn source and the Sb source in the mixed solution: citric acid:ethylene glycol=1:3:10;

[0060] (3) The electrode was prepared by complete immersion and coating according to the method in step (3) of Example 1 to obtain a Ti / SnO2-Sb electrode.

[0061] Comparative Example 2

[0062] A method for preparing a Ti / SnO2-Sb-Ho electrode comprises the following steps:

[0063] (1) The pretreatment of the electrode substrate was carried out according to the method of Example 1;

[0064] (2) placing ethylene glycol in a water bath and heating it to 65°C, then adding citric acid and stirring until completely dissolved to obtain a citric acid ethylene glycol solution; then heating it to 90°C, adding tin tetrachloride (SnCl4), antimony trichloride SbCl3 and holmium nitrate (Ho·3NO3·5H2O) to the organic solvent in a molar ratio of Sn:Sb:Ho=100:10:1.5, heating and stirring in a 90°C constant temperature water bath until dissolved to obtain a mixed solution, and after cooling, ultrasonicating the mixed solution at 100 Hz for 15 minutes to obtain a Sn-Sb-Ho sol; wherein the total molar number of the Sn source and the Sb source in the mixed solution: citric acid:ethylene glycol=1:3:10;

[0065] (3) The electrode was prepared by complete immersion and coating according to the method in step (3) of Example 1 to obtain a Ti / SnO2-Sb-Ho electrode.

[0066] Test example

[0067] 1. The high-activity Ti / SnO2-Sb-Tb electrode prepared in Example 1 and the Ti / SnO2-Sb electrode prepared in Comparative Example 1 were subjected to surface electron microscopy (SEM). The photographs magnified 1000 times and 200 times are shown as follows: Figure 1 shown.

[0068] pass Figure 1 a and Figure 1A comparison of Example 1 and Comparative Example 1 reveals significant differences in morphology and structure between the high-activity Ti / SnO2-Sb-Tb electrode prepared in Example 1 and Comparative Example 1. The conventional Ti / SnO2-Sb electrode has an uneven surface, with large crystal particles in most areas and clustering. In contrast, the high-activity Ti / SnO2-Sb-Tb electrode in Example 1 exhibits a dense coating that is evenly distributed and well-dispersed across the surface, with no clustering.

[0069] pass Figure 1 c and Figure 1 By comparison with d, it can be found that no obvious active sites are generated on the surface of the traditional Ti / SnO2-Sb electrode in comparative example 1, while uniform active grain sites are generated on the surface of the high-activity Ti / SnO2-Sb-Tb electrode in embodiment 1.

[0070] Therefore, the present invention dopes the rare earth element Tb into the Ti / SnO2-Sb electrode and adopts Tb-Sn-Sb sol coating to obtain a Ti / SnO2-Sb electrode coating with a denser and more uniform surface, higher surface crystallinity of the electrode, smaller grain size, and increased specific surface area of ​​the electrode, thereby increasing the contact between the electrode and the target pollutant, improving the conductivity of the electrode, improving the performance of the electrode, improving the electrocatalytic activity of the electrode, and extending the service life of the electrode.

[0071] 2. The high-activity Ti / SnO2-Sb-Tb electrode prepared in Example 1 and the Ti / SnO2-Sb electrode prepared in Comparative Example 1 were subjected to X-ray diffraction (XRD) analysis. The obtained patterns are as follows: Figure 2 shown.

[0072] Depend on Figure 2 It can be seen that the diffraction peak intensity of the high-activity Ti / SnO2-Sb-Tb electrode doped with rare earth element Tb is weaker than that of the undoped electrode, which results in lattice expansion. The reason is that the Tb with larger ion radius 3+ Entering the SnO2 lattice to replace Sn 4+ The diffraction peak of the Tb-doped modified electrode is slightly wider. Since the average grain size is inversely proportional to the diffraction peak width, this indicates that the SnO2 grains in the coating are smaller than those in the blank electrode. This indicates that Tb-doping refines the SnO2 grains in the coating, increasing the specific surface area for electrocatalytic reactions and improving the electrocatalytic performance of the Tb-doped modified electrode. The conclusions drawn from the XRD pattern are consistent with those observed in the SEM images and the actual degradation results.

[0073] 3. The high-activity Ti / SnO2-Sb-Tb electrode prepared in Example 1, the Ti / SnO2-Sb electrode prepared in Comparative Example 1, and the Ti / SnO2-Sb-Ho electrode prepared in Comparative Example 2 were tested for electrochemical electrocatalytic degradation of moxifloxacin (MOX) solution.

[0074] The test conditions are as follows: the anode is the highly active Ti / SnO2-Sb-Tb electrode of Example 1, the Ti / SnO2-Sb electrode of Comparative Example 1, and the Ti / SnO2-Sb-Ho electrode of Comparative Example 2; the cathode is a pure titanium plate; the electrolyte is a Na2SO4 solution containing 0.05 mol / L; the concentration of the target pollutant moxifloxacin is 100 mg / L; the pH value is 6.5 under the initial conditions; and the current density is 20 mA / cm 2 , the effective electrolysis area is 30mmx40mm, the electrolysis time is 30min, the test results are as follows Figure 3 shown.

[0075] Depend on Figure 3 It can be seen that the highly active Ti / SnO2-Sb-Tb electrode of Example 1 of the present invention achieves a moxifloxacin (MOX) removal rate of over 84%, while the conventional Ti / SnO2-Sb electrode of Comparative Example 1 achieves a moxifloxacin (MOX) removal rate of only 58.4%, and the Ho-doped Ti / SnO2-Sb-Ho electrode of Comparative Example 2 achieves a moxifloxacin (MOX) removal rate of 74.1%. This means that the Ti / SnO2-Sb-Tb electrode of Example 1 improves the moxifloxacin (MOX) removal rate by 9.9-25.6% compared to Comparative Examples 1-2. This fully demonstrates that the highly active Ti / SnO2-Sb-Tb electrode of Example 1 has a strong ability to degrade organic pollutants. Specifically, doping the Ti / SnO2-Sb electrode with the rare earth element Tb can significantly enhance the electrode's electrocatalytic degradation effect, electrocatalytic activity, and ability to treat wastewater containing organic pollutants.

Claims

1. A method for preparing a highly active titanium-based tin dioxide-antimony electrode, characterized in that: The steps include: (1) adding Sn source, Sb source and Tb source to an organic solvent to prepare a mixed solution, wherein the ion molar concentration ratio of the Sn source, Sb source and Tb source in the mixed solution is Sn:Sb:Tb=100:10:(0.1-2); then ultrasonicating the mixed solution at 50-150 Hz for 10-20 min, standing and aging for 1-2 h, to obtain a Tb-Sn-Sb sol; (2) completely immersing the pretreated electrode substrate in the Tb-Sn-Sb sol obtained in step (1), taking it out and evenly applying the Tb-Sn-Sb sol on the surface of the electrode substrate with a soft brush, then drying the coated electrode substrate at 100-130° C. for 10-20 min, and then heat treating it at 450-600° C. for 10-30 min, taking it out and cooling it to room temperature, washing the surface with deionized water, and drying it; (3) Repeat the complete immersion and coating of step (2) 5 to 9 times, dry the electrode substrate after the last complete immersion and coating at 100 to 130° C. for 10 to 20 minutes, and then calcine at 550 to 700° C. for 1 to 2 hours. After taking out, cool to room temperature, clean the surface with deionized water and dry to obtain a highly active titanium-based tin dioxide-antimony electrode.

2. The preparation method according to claim 1, characterized in that In step (1), the Sn source is crystalline tin tetrachloride, the Sb source is antimony trichloride, and the Tb source is terbium nitrate.

3. The preparation method according to claim 1, characterized in that: In step (1), the organic solvent is a citric acid ethylene glycol solution, and the total molar number of the Sn source and the Sb source in the mixed solution is: citric acid: ethylene glycol = 1: (2-5): (8-12); Further preferably, the organic solvent is an ethylene glycol solution of citric acid, and the total molar number of the Sn source and the Sb source in the mixed solution: citric acid:ethylene glycol=1:3:

10.

4. The preparation method according to claim 1, characterized in that: In step (1), the ion molar concentration ratio of the Sn source, Sb source and Tb source is Sn:Sb:Tb=100: 10:1.5。 5. The preparation method according to claim 1, characterized in that: In step (2), the electrode substrate is a titanium mesh, and the pretreatment method thereof is: after polishing, alkali washing, and acid washing in sequence, ultrasonic cleaning at 100 Hz for 10 minutes, and then cleaning with deionized water, placing it in an oven to dry, and the pretreated electrode substrate is stored in anhydrous ethanol.

6. The preparation method according to claim 1, characterized in that: In step (2), the coated electrode substrate is placed in an electric hot air drying oven and dried at 130° C. for 20 minutes, and then placed in a muffle furnace and heat treated at 500° C. for 20 minutes.

7. The preparation method according to claim 1, characterized in that: In step (3), the complete immersion and coating are repeated 6 times. After the last coating, the electrode substrate is placed in an electric hot air drying oven and dried at 130°C for 20 minutes, then placed in a muffle furnace and baked at 600°C for 2 hours, and then taken out and cooled to room temperature.

8. A highly active titanium-based tin dioxide-antimony electrode, characterized in that: It is prepared according to the preparation method according to any one of claims 1 to 7.

9. Use of the high-activity titanium-based tin dioxide-antimony electrode described in claim 1 in treating wastewater containing organic pollutants.

10. The use according to claim 9, characterized in that The organic pollutant is a fluoroquinolone antibiotic.

Citation Information

Patent Citations

  • Preparation method of neodymium-doped titanium base tin dioxide-antimony electrode

    CN101654790A

  • Preparation method of titanium-based tin dioxide-antimony electrode with compact and uniform electrode coating

    CN113233550A

  • Rare-earth doped titanium-base SnO2 electrolytic electrode and its preparation

    CN1896320A

  • Electrode and its manufacturing method using rareearth element

    KR1020030080536A