Scratch-resistant and wear-resistant AG microcrystalline glass as well as preparation method and application thereof
By treating the surface of microcrystalline glass with a horizontal sandblasting machine and acid washing and polishing process, the problem of poor scratch resistance in the existing technology has been solved, and the preparation of scratch-resistant AG microcrystalline glass has been realized, which is suitable for household appliance panels and reduces the preparation cost.
Patent Information
- Application Number
- CN202411014304.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-26
- Publication Date
- 2024-11-22
Abstract
Description
Technical Field
[0001] The present invention relates to the field of glass-ceramic processing, and in particular to a scratch-resistant AG glass-ceramic and a preparation method and application thereof. Background Art
[0002] Glass-ceramics, also known as glass ceramics, is a material with a microcrystalline phase formed by special processing of glass. It combines the advantages of glass and ceramics, such as high mechanical strength, good thermal stability, and chemical corrosion resistance, which makes it widely used in many fields, especially in the manufacture of high-end home appliances and electronic products. Etched AG glass-ceramics technology is a surface treatment process that forms a uniform AG (Anti-Glare, anti-glare) etching coating on the surface of glass-ceramics by sandblasting and acid etching. The surface of the AG etching coating presents a slight roughness, which helps to scatter reflected light, reduce glare and fingerprints, and maintain high light transmittance. This treatment can significantly improve the surface texture and visual effect of glass-ceramics, reduce direct reflection of light, and provide users with a more comfortable visual experience.
[0003] However, the surface scratch resistance of the microcrystalline glass obtained by the current AG microcrystalline glass surface treatment technology is poor. Summary of the invention
[0004] In view of the above-mentioned deficiencies in the prior art, the present invention proposes a scratch-resistant AG microcrystalline glass and a preparation method and application thereof, aiming to solve the problem of poor surface scratch resistance of microcrystalline glass obtained by current AG microcrystalline glass surface treatment technology.
[0005] To achieve the above-mentioned purpose, the present invention proposes a method for preparing scratch-resistant AG microcrystalline glass, comprising the following steps: S1: cleaning the original microcrystalline glass sheet and drying it without polishing and edge grinding pretreatment; S2: passing the dried microcrystalline glass through a horizontal sandblasting machine to obtain sandblasted microcrystalline glass; S3: pickling, grinding and cleaning the sandblasted microcrystalline glass, and then repeating the steps of "pickling, grinding and cleaning" 2 to 8 times, and drying to obtain scratch-resistant AG microcrystalline glass.
[0006] Optionally, the drying temperature is 30°C to 40°C.
[0007] Optionally, the rotation speed of the horizontal sand blasting machine is 600 rpm to 900 rpm.
[0008] Optionally, the step of using a horizontal sand blasting machine includes: using 35-mesh to 45-mesh corundum to sand the surface of the microcrystalline glass for 30 minutes to 40 minutes.
[0009] Optionally, the pickling and polishing includes: the pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it.
[0010] Optionally, the reagents used in the pickling and polishing include, by weight: 20-30 parts of water, 15-25 parts of ammonium sulfate, 20-30 parts of barium sulfate, 12-16 parts of oxalic acid and 15-18 parts of ammonium acetofluoride.
[0011] Optionally, the spraying is achieved by a pump, and the pressure of the pump is 0.2Mpa to 0.5Mpa.
[0012] Optionally, the grinding time is 6 minutes to 8 minutes.
[0013] In order to achieve the above object, the present invention also provides a scratch-resistant AG microcrystalline glass prepared by the above method.
[0014] In order to achieve the above-mentioned purpose, the present invention also proposes an application of scratch-resistant AG microcrystalline glass, wherein the scratch-resistant AG microcrystalline glass is applied to household appliances, and the household appliances include one of an induction cooker, an electric ceramic stove, a microwave oven, a gas stove, and a tea stove.
[0015] Beneficial effects of the present invention: The method for preparing the scratch-resistant AG microcrystalline glass provided by the present invention does not use the sandblasting process to avoid the generation of burrs in the process of spraying brown corundum (sand) on the surface of the glass with high pressure, but adopts a horizontal sandblasting machine and a grinding process in combination, and prepares an acid pickling agent. By surface treating the microcrystalline glass original sheet, a microcrystalline glass with a surface that is more scratch-resistant and anti-fingerprint is obtained, which can be used in the panel of household appliances without being scratched and greatly saves the preparation cost. DETAILED DESCRIPTION
[0016] In order to make the purpose, technical solutions and advantages of the embodiments of the present invention clearer, the technical solutions in the embodiments of the present invention will be clearly and completely described below. It should be understood that the following embodiments are only used to explain the present invention and are not used to limit the present invention.
[0017] Unless defined otherwise, all technical and scientific terms used herein have the common meaning in the art to which the claimed subject matter pertains.
[0018] It should be noted that if the embodiments of the present invention involve directional indications (such as up, down, left, right, front, back, etc.), the directional indications are only used to explain the relative position relationship, movement status, etc. between the components in a certain specific posture. If the specific posture changes, the directional indication will also change accordingly.
[0019] In addition, if there are descriptions involving "first", "second", etc. in the embodiments of the present invention, the descriptions of "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of technical features indicated. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, if the meaning of "and / or" appearing in the full text is to include three parallel schemes, taking "A and / or B" as an example, it includes scheme A, or scheme B, or a scheme that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0020] Glass-ceramics, also known as glass ceramics, is a material with a microcrystalline phase formed by special processing of glass. It combines the advantages of glass and ceramics, such as high mechanical strength, good thermal stability, and chemical corrosion resistance, which makes it widely used in many fields, especially in the manufacture of high-end home appliances and electronic products. Etched AG glass-ceramics technology is a surface treatment process that forms a uniform AG (Anti-Glare, anti-glare) etching coating on the surface of glass-ceramics by sandblasting and acid etching. The surface of the AG etching coating presents a slight roughness, which helps to scatter reflected light, reduce glare and fingerprints, and maintain high light transmittance. This treatment can significantly improve the surface texture and visual effect of glass-ceramics, reduce direct reflection of light, and provide users with a more comfortable visual experience.
[0021] However, the surface scratch resistance of the microcrystalline glass obtained by the current AG microcrystalline glass surface treatment technology is poor.
[0022] In order to solve the above problems, the present invention provides a method for preparing scratch-resistant AG glass-ceramics, comprising the following steps:
[0023] S1: cleaning the glass-ceramics and drying it;
[0024] In this scheme, cleaning includes placing the microcrystalline glass on the track of the plate washer, adjusting the speed of the plate washer to between 2-5, then opening the water tap of the plate washer, and then turning on the drying switch for drying.
[0025] S2: passing the dried micro-ceramics through a horizontal sandblasting machine to obtain sandblasted micro-ceramics;
[0026] In this solution, the horizontal glass sandblasting machine is directly driven by a motor. The sandblasting wheel installed on the main shaft is used to hit the dust-free corundum sand on the glass surface at high speed. Compared with sandblasting, it can achieve the desired effect more gently.
[0027] From the perspective of energy saving, in some embodiments, the average power of a small horizontal glass sandblasting machine is 3.8kw. The vertical sandblasting machine normally operates 3 guns and requires a 12kw air compressor. In addition, the machine itself consumes 3.8kw of electricity. The vertical sandblasting machine consumes more than 15kw of electricity per hour. In this way, the horizontal glass sandblasting machine saves 12kw of electricity than the vertical sandblasting machine. If it works 8 hours a day, it can save electricity bills (12kw*8 hours=96 yuan) (electricity bills are calculated at 1 yuan per 1kw). It can be concluded that the horizontal glass sandblasting machine can save more than 30,000 yuan in electricity bills a year, greatly saving costs.
[0028] S3: The sandblasted microcrystalline glass is pickled, polished and then cleaned, and then the steps of "pickling, polishing and then cleaning" are repeated 2 to 8 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0029] In some embodiments, the step of "cleaning after pickling and polishing" is preferably repeated 4 to 6 times.
[0030] Furthermore, the drying temperature is 30°C to 40°C.
[0031] In some embodiments of the present scheme, the drying temperature is any value between 30°C and 40°C, such as 30°C, 32°C, 34°C, 36°C, 38°C, and 40°C. Drying within this temperature range is beneficial to ensure the surface activity of the microcrystalline glass after contact with the pickling agent in the next step of surface treatment.
[0032] Furthermore, the rotation speed of the horizontal sand blasting machine is 600 rpm to 900 rpm.
[0033] The rotation speed of the sandblasting machine affects the speed at which the sand belt contacts the glass, thereby affecting the grinding efficiency and surface quality. In some embodiments of the present solution, the rotation speed of the horizontal sandblasting machine is any value between 600 rpm and 900 rpm, such as 600 rpm, 700 rpm, 800 rpm, and 900 rpm.
[0034] Furthermore, the step of using a horizontal sandblasting machine includes: sanding the surface of the microcrystalline glass for 30 minutes to 40 minutes using 35-45 mesh corundum. The grit number determines the grain size of the sand belt, that is, the size of the abrasive grains on the surface of the sand belt. The grit number of this solution is relatively low and is used for rough grinding.
[0035] In some embodiments of the present scheme, the mesh number of the corundum is 35 mesh, 40 mesh, 45 mesh, or any value between 35 mesh and 45 mesh.
[0036] Furthermore, the pickling and polishing includes: the pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. In one embodiment, the adjusted reaction reagent is sprayed onto the surface of the microcrystalline glass using the automatic horizontal spraying and friction method of the pickling professional equipment, and the equipment transfers the microcrystalline glass to the reagent reaction area for polishing. Pickling and polishing can significantly improve the surface properties of the microcrystalline glass, including reducing the surface roughness, eliminating tiny cracks and defects, and thus improving the optical and mechanical properties of the material.
[0037] Furthermore, the reagents used in the pickling and polishing include, by weight: 20 to 30 parts of water, 15 to 25 parts of ammonium sulfate, 20 to 30 parts of barium sulfate, 12 to 16 parts of oxalic acid and 15 to 18 parts of ammonium acetofluoride.
[0038] In some embodiments, the pickling and polishing reagent also includes hydrofluoric acid and chromic acid. After the microcrystalline glass passes through the pickling reaction reagent, the hydrofluoric acid (HF) in the reaction reagent reacts with silicon dioxide (SiO2), the main component of the microcrystalline glass. The reaction formula is as follows: SiO2+6HF→H2SiF6+2H2OSiO2+6HF→
[0039] H2SiF6+2H2O. In this reaction, SiO2 reacts with HF to form hexafluorosilicic acid (H2SiF6) and water. Since hexafluorosilicic acid is in liquid form, it can be dissolved in an acidic solution and will not leave solid residues on the glass surface, thus avoiding surface contamination during the reaction. Since glass-ceramics also contain other metal oxides (such as boron, aluminum, lithium, etc.), these components will also react with hydrofluoric acid. Glass-ceramics containing aluminum may undergo the following reaction: Al2O3+6HF→
[0040] 2AlF3+3H2OAl2O3+6HF→2AlF3+3H2O.
[0041] The use of the above pickling reagent, in combination with the polishing process of this solution, can synergistically treat the surface of the microcrystalline glass to achieve a higher wear resistance.
[0042] Furthermore, the spraying is achieved by a pump, and the pressure of the pump is 0.2Mpa to 0.5Mpa.
[0043] Spraying the pickling agent within the above pressure range can achieve uniform and efficient spraying and avoid damage to the surface of the microcrystalline glass. In some embodiments, the pressure of the pump is any value between 0.2Mpa and 0.5Mpa, such as 0.2Mpa, 0.3Mpa, 0.4Mpa, and 0.5Mpa.
[0044] Furthermore, the grinding time is 6 minutes to 8 minutes. In some embodiments, the grinding time is any value between 6 minutes and 8 minutes, such as 6 minutes, 7 minutes, and 8 minutes. In some embodiments, the cleaning reagent used in the cleaning step after grinding includes plasma water, sodium carbonate and sodium polyphosphate, and the obtained glass does not need to be specially cleaned, but only needs to be passed through an ordinary plate washer.
[0045] In order to solve the above problems, the present invention also proposes a scratch-resistant AG microcrystalline glass prepared by the above preparation method. The scratch-resistant AG microcrystalline glass has no burrs, excellent surface mechanical properties, and is not easy to be scratched or worn.
[0046] To solve the above problems, the present invention also proposes an application of scratch-resistant AG micro-ceramic glass, which is applied to household appliances, including one of an induction cooker, an electric ceramic cooker, a microwave oven, a gas stove, and a tea stove. The micro-ceramic glass of this solution is suitable for manufacturing a stove panel due to its wear resistance, corrosion resistance, and high temperature resistance, and can be directly heated on the table for cooking.
[0047] Embodiment 1:
[0048] Place the glass-ceramic on the plate washer track, adjust the plate washer speed to between 2-5, then open the water tap of the plate washer, and then turn on the drying switch for drying. The drying temperature is 35°C.
[0049] The dried micro-ceramics are passed through a horizontal sand blasting machine, the rotation speed of the horizontal sand blasting machine is 800 rpm, and 40-mesh corundum is used to sand the surface of the micro-ceramics for 40 minutes to obtain the micro-ceramics after sand blasting;
[0050] The sandblasted microcrystalline glass is pickled, polished and then cleaned. The pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. The spraying is achieved by a pump with a pressure of 0.2Mpa. The reagents used include: 25 parts of water, 20 parts of ammonium sulfate, 25 parts of barium sulfate, 15 parts of oxalic acid and 17 parts of ammonium acetofluoride. The polishing time is 7 minutes, and then the steps of "pickling, polishing and cleaning" are repeated 6 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0051] Embodiment 2:
[0052] Place the glass-ceramic on the plate washer track, adjust the plate washer speed to between 2-5, then open the water tap of the plate washer, and then turn on the drying switch for drying. The drying temperature is 35°C.
[0053] The dried microcrystalline glass is passed through a horizontal sandblasting machine with a rotation speed of 800 rpm. 35-mesh corundum is used to sand the surface of the microcrystalline glass for 40 minutes to obtain the sandblasted microcrystalline glass; the sandblasted microcrystalline glass is pickled and polished and then cleaned. The pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. The spraying is achieved by a pump with a pressure of 0.2 MPa. The reagents used include: 25 parts of water, 15 parts of ammonium sulfate, 30 parts of barium sulfate, 15 parts of oxalic acid and 18 parts of ammonium acetofluoride. The polishing time is 8 minutes, and then the step of "cleaning after pickling and polishing" is repeated 4 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0054] Embodiment 3:
[0055] Place the glass-ceramic on the plate washer track, adjust the plate washer speed to between 2-5, then open the water tap of the plate washer, and then turn on the drying switch for drying. The drying temperature is 35°C.
[0056] The dried microcrystalline glass is passed through a horizontal sandblasting machine with a rotation speed of 800 rpm. 35-mesh corundum is used to sand the surface of the microcrystalline glass for 40 minutes to obtain the sandblasted microcrystalline glass; the sandblasted microcrystalline glass is pickled and polished and then cleaned. The pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. The spraying is achieved by a pump with a pressure of 0.2 MPa. The reagents used include: 25 parts of water, 15 parts of ammonium sulfate, 30 parts of barium sulfate, 15 parts of oxalic acid and 18 parts of ammonium acetofluoride. The polishing time is 8 minutes, and then the step of "cleaning after pickling and polishing" is repeated 4 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0057] Embodiment 4:
[0058] Place the glass-ceramic on the plate washer track, adjust the plate washer speed to between 2-5, then open the water tap of the plate washer, and then turn on the drying switch for drying. The drying temperature is 40℃;
[0059] The dried micro-ceramic glass is passed through a horizontal sand blasting machine, the rotation speed of the horizontal sand blasting machine is 800 rpm, and 35-mesh corundum is used to sand the surface of the micro-ceramic glass for 40 minutes to obtain the micro-ceramic glass after sand blasting;
[0060] The sandblasted microcrystalline glass is pickled, polished and then cleaned. The pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. The spraying is achieved by a pump with a pressure of 0.5Mpa. The reagents used include: 20 parts of water, 15 parts of ammonium sulfate, 20 parts of barium sulfate, 12 parts of oxalic acid and 18 parts of ammonium acetofluoride. The polishing time is 6 minutes, and then the steps of "pickling, polishing and cleaning" are repeated 8 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0061] Comparative Example 1:
[0062] Place the glass-ceramic on the plate washer track, adjust the plate washer speed to between 2-5, then open the water tap of the plate washer, and then turn on the drying switch for drying. The drying temperature is 40℃;
[0063] Passing the dried micro-ceramic glass through a vertical sandblasting machine to obtain sandblasted micro-ceramic glass;
[0064] The sandblasted microcrystalline glass is pickled, polished and then cleaned. The pickling equipment sprays the reagent on the surface of the microcrystalline glass, and then polishes it. The spraying is achieved by a pump with a pressure of 0.5Mpa. The reagents used include: 30 parts of water, 25 parts of ammonium sulfate, 20 parts of barium sulfate, 10 parts of oxalic acid and 30 parts of ammonium acetofluoride. The polishing time is 6 minutes, and then the steps of "pickling, polishing and cleaning" are repeated 5 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
[0065] Furthermore, the glass-ceramics finally prepared in Examples 1 to 4 and Comparative Example 1 were used for performance testing, including Mohs hardness, water drop angle and wear resistance. The results are shown in Table 1 below:
[0066] Table 1.
[0067] Mohs hardness Water drop angle Wear resistance comparison Example 1 8H 116.920 0 Example 2 8H 118.380 0 Example 3 8H 115.443 0 Example 4 8H 117.567 0 Comparative Example 1 6.5H 78.567 90%
[0068] According to this table, it can be confirmed that the process of this solution: 1. Improvement of the hardness performance of microcrystalline glass: The Mohs hardness of the surface of the microcrystalline glass without acid washing and polishing is 6.5H, and the Mohs hardness test of the surface of the microcrystalline glass after sanding and acid washing and polishing is 8H, and the surface hardness is enhanced and the scratch resistance is improved; 2. Improvement of the water drop angle of the surface of the microcrystalline glass: The water drop angle of the surface of the microcrystalline glass without sanding and acid polishing is 78.567, and the overall average water drop angle of the surface of the microcrystalline glass after sanding and acid polishing is 117.0775. The overall water drop angle is greater than 110° for the best effect; 3. Comparison of the wear resistance coefficient of the microcrystalline board Rising: Clean steel wool was used to repeatedly rub the surface of the microcrystalline glass. 9 out of 10 microcrystalline glass were scratched. Similarly, the steel wool was used to repeatedly rub the surface of the microcrystalline glass after sandblasting and acid polishing. None of the 10 scratch-resistant glass were scratched. This solution uses a horizontal sandblasting machine and a polishing process, and mixes pickling reagents. By treating the surface of the original microcrystalline glass, a microcrystalline glass with a more scratch-resistant and anti-fingerprint surface is obtained, which can be used in the panel of household appliances without being scratched, and greatly saves the preparation cost.
[0069] The above are only preferred embodiments of the present invention, and do not limit the patent scope of the present invention. For those skilled in the art, the present invention may have various changes and modifications. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.
Claims
1. A method for preparing scratch-resistant AG glass-ceramics, It is characterized in that The following steps are involved: S1: After cleaning the original glass-ceramic sheet, it is dried without polishing or edge grinding pretreatment; S2: passing the dried micro-ceramics through a horizontal sandblasting machine to obtain sandblasted micro-ceramics; S3: The sandblasted microcrystalline glass is pickled, polished and then cleaned, and then the steps of "pickling, polishing and then cleaning" are repeated 2 to 8 times, and then dried to obtain scratch-resistant AG microcrystalline glass.
2. The method for preparing the scratch-resistant AG glass-ceramics according to claim 1, It is characterized in that The drying temperature is 30°C to 40°C.
3. The method for preparing the scratch-resistant AG glass-ceramics according to claim 1, It is characterized in that The rotation speed of the horizontal sand blasting machine is 600 rpm to 900 rpm.
4. The method for preparing the scratch-resistant AG glass-ceramics according to claim 1, It is characterized in that The step of using a horizontal sand blasting machine includes: using 35-mesh to 45-mesh corundum to sand the surface of the microcrystalline glass for 5 minutes to 10 minutes.
5. The method for preparing the scratch-resistant AG glass-ceramics according to claim 1, It is characterized in that The pickling and polishing process comprises: the pickling equipment sprays reagents on the surface of the microcrystalline glass, and then polishes.
6. The method for preparing the scratch-resistant AG glass-ceramics according to claim 5, It is characterized in that In parts by weight, the reagents used in the pickling and polishing include: 20-30 parts of water, 15-25 parts of ammonium sulfate, 20-30 parts of barium sulfate, 12-16 parts of oxalic acid and 15-18 parts of ammonium acetofluoride.
7. The method for preparing the scratch-resistant AG glass-ceramics according to claim 5, It is characterized in that The spraying is achieved by a pump, and the pressure of the pump is 0.2Mpa to 0.5Mpa.
8. The method for preparing the scratch-resistant AG glass-ceramics according to claim 5, It is characterized in that The grinding time is 6 to 8 minutes.
9. A scratch-resistant AG glass-ceramic. It is characterized in that The invention comprises the scratch-resistant AG microcrystalline glass prepared by the preparation method according to any one of claims 1 to 8.
10. An application of the scratch-resistant AG glass-ceramic as claimed in claim 9, It is characterized in that The scratch-resistant AG microcrystalline glass is applied to household appliances, which include an induction cooker, an electric ceramic cooker, a microwave oven, a gas stove, and a tea stove.
Citation Information
Patent Citations
Preparation method for glass used on mobile phone screen
CN104445978A
Processing technology of frosted glass
CN107088827A
Frosted treatment process of glass surface
CN110655333A
Preparation process of antiskid glass base plate
CN111138083A
Ceramic-based glass manufacturing process
CN111233343A
Cited By
Easy-to-clean microcrystalline glass and preparation method thereof
CN120921176A
A kind of easy-to-clean microcrystalline glass and its preparation method
CN122938680A