Preparation method and preparation device of large-area and high-performance electrochromic film

Tungsten oxide and Prussian blue films were prepared on transparent conductive substrates by chemical bath deposition. The citrate compound was used to ensure deposition uniformity and morphology control, which solved the problems of high cost and poor uniformity in the prior art, and achieved large area and high Preparation of performance electrochromic films, suitable for industrial applications.

CN118993565APending Publication Date: 2024-11-22ZHEJIANG UNIV +1

Patent Information

Application Number
CN202411078463.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-07
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The existing electrochromic film preparation methods have problems such as high cost, complex equipment and poor uniformity in large areas. In particular, the high temperature and high pressure conditions of hydrothermal method restrict large-scale preparation, and it is difficult for the electrodeposition method to control the electric field distribution and affect the uniformity of the film.

Method used

Using chemical bath deposition method, tungsten oxide and Prussian blue films were prepared on a transparent conductive substrate by using a mixed aqueous solution of tungstate and citrate compound and a mixed aqueous solution of iron salt and citrate compound as a precursor. , use citrate compounds to ensure deposition uniformity and morphological control, and achieve low-cost large-area preparation.

Benefits of technology

It has achieved the preparation of low-cost, large-area and high-performance electrochromic films, with good film uniformity and high overlap in transmittance curves, which are suitable for industrial applications. The electrochromic performance of tungsten oxide and Prussian blue is significantly improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993565A_ABST
    Figure CN118993565A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method and a preparation device of a large-area and high-performance electrochromic film, and belongs to the field of electrochromic films, the method comprises the following steps: (1) preparing a precursor solution which comprises a solution A and a solution B; (2) placing a transparent conductive substrate in a reaction chamber, adding the solution A and the solution B at the same time, performing chemical bath deposition to obtain a precursor film, and performing post-treatment on the precursor film to obtain the large-area and high-performance electrochromic film, when the prepared electrochromic film is a tungsten oxide film, the solution A is a mixed aqueous solution of tungstate and citrate, and the solution B is hydrochloric acid; when the prepared electrochromic film is a Prussian blue film, the solution A is a mixed aqueous solution of ferric salt and citrate, and the solution B is a potassium ferricyanide aqueous solution. The method has the advantages of simple and mild process conditions and low preparation cost, can realize large-area uniform preparation of tungsten oxide and Prussian blue films, and has a wide prospect in practical industrial application.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the field of electrochromic films, and in particular to a preparation method and a preparation device for a large-area, high-performance electrochromic film. Background Art

[0002] Electrochromic glass can display reversible changes in color and transparency under the action of a small external voltage, dynamically regulating the sunlight and heat entering the room, thereby significantly reducing the energy consumption of indoor cooling, heating or lighting systems, and has broad application prospects in the field of building energy conservation. At present, the preparation of electrochromic glass in industry is mainly through physical sputtering methods represented by magnetron sputtering, which is layer-by-layer deposition. However, the physical sputtering process requires complex equipment and strict vacuum conditions, and the preparation cost is very high, which also makes it difficult to promote and apply electrochromic technology on a large scale.

[0003] The conditions for preparing electrochromic films by wet chemical methods are relatively mild, which can effectively reduce the preparation cost. Currently, wet chemical methods such as sol-gel method, spray pyrolysis method, hydrothermal method, and electrodeposition method have been used to prepare electrochromic films, but they all have corresponding preparation or performance disadvantages. For example, the films prepared by sol-gel method and spray pyrolysis method generally present a dense morphology, which is not conducive to the reversible embedding / de-embedding of ions, thereby affecting the electrochromic properties of the film. The hydrothermal method is limited in large-scale preparation due to its high temperature and high pressure reaction conditions. The electric field distribution that is difficult to control in the electrodeposition method will also affect the uniformity of the film during large-area preparation.

[0004] The Chinese patent document with publication number CN106399979A discloses a method for preparing a flower-like WO3 thin film for electrochromic change, wherein the tungsten concentration is 0.03-0.05 mol·L -1 Add NaCl as a stabilizer to the aqueous solution, stir until transparent, and then add 1 mol·L -1 The pH value was adjusted to 3 by hydrochloric acid; CTAB was then added as a surfactant, and a yellow-green solution was obtained as a WO3 precursor solution after stirring for a period of time. Then, WO3 was prepared on FTO conductive glass by hydrothermal method (maintained at 180°C for 24 hours), and after washing and drying, it was placed in a muffle furnace for annealing to obtain a cluster-shaped WO3 film. However, as mentioned above, the high temperature and high pressure preparation conditions of the hydrothermal method limit the large-scale preparation of the product film.

[0005] The Chinese patent document with publication number CN113867065A discloses a method for preparing a Prussian blue electrochromic film. The method first dissolves ferrocyanide, trivalent iron salt and potassium salt in deionized water to obtain a uniform solution; the conductive substrate is electrically contacted with the metal and immersed in the uniform solution obtained in the above steps for reaction. After the reaction is completed, a layer of Prussian blue electrochromic film is formed in situ on the surface of the conductive substrate. The invention adopts the electrodeposition method, and the prepared film has poor adhesion and poor cycle stability. It has certain requirements for the electrical properties of the substrate and has high requirements for electric field uniformity for large-area preparation. Summary of the invention

[0006] In order to solve the problems of harsh preparation conditions and poor uniformity over a large area of ​​the existing electrochromic film, the present invention provides a preparation method and a preparation device for a large-area, high-performance electrochromic film.

[0007] The specific technical solutions adopted are as follows:

[0008] A method for preparing a large-area, high-performance electrochromic film comprises the following steps:

[0009] (1) preparing a precursor solution required for a chemical bath deposition reaction, wherein the precursor solution includes a solution A and a solution B;

[0010] (2) placing a transparent conductive substrate in a reaction chamber, adding solution A and solution B at the same time, performing chemical bath deposition to obtain a precursor film, and performing post-treatment on the precursor film to obtain the large-area, high-performance electrochromic film;

[0011] When the electrochromic film is a tungsten oxide film, solution A is a mixed aqueous solution of tungstate and a citrate-containing compound, solution B is hydrochloric acid, and the post-treatment step is an annealing process;

[0012] When the prepared electrochromic film is a Prussian blue film, solution A is a mixed aqueous solution of iron salt and a citrate-containing compound, solution B is an aqueous solution of potassium ferrocyanide, and the post-treatment step is a drying process.

[0013] The method of the present invention utilizes mild reaction conditions of chemical bath deposition and simple deposition equipment to realize low-cost, large-area preparation of cathode tungsten oxide thin films and anode Prussian blue thin films, and the method of the present invention can be used for the preparation of cathode tungsten oxide thin films as well as the preparation of anode Prussian blue thin films. Citrate ensures the uniformity of thin film deposition on the substrate, and at the same time, the nanosheet morphology of tungsten oxide prepared by the method of the present invention shortens the ion diffusion distance in the electrochromic reaction and provides more reactive sites; the metal organic framework structure of Prussian blue prepared by the method of the present invention provides a stable ion transmission channel, and its reversible conversion from blue to colorless ensures the coordination of Prussian blue and tungsten oxide in the electrochromic process.

[0014] The transparent conductive substrate includes but is not limited to ITO transparent conductive glass, FTO transparent conductive glass, AZO transparent conductive glass, GZO transparent conductive glass, metal nanowire network transparent electrode, etc.

[0015] Preferably, the transparent conductive substrate is ultrasonically cleaned before the precursor film is deposited.

[0016] Preferably, when the electrochromic film obtained is a tungsten oxide film, solution A is a mixed aqueous solution of sodium tungstate and sodium citrate or a mixed aqueous solution of sodium tungstate and citric acid; when the electrochromic film obtained is a Prussian blue film, solution A is a mixed aqueous solution of ferric chloride and sodium citrate or a mixed aqueous solution of ferric chloride and citric acid.

[0017] Preferably, when the prepared electrochromic film is a tungsten oxide film, solution A is a mixed aqueous solution of sodium tungstate and sodium citrate, the concentration of sodium tungstate is 0.01-0.1M, more preferably 0.03M, the molar ratio of sodium citrate to sodium tungstate is 1.5-3.5:1, more preferably 2:1, the hydrochloric acid concentration of solution B is 1-5M, more preferably 3M, and the volume ratio of solution A to solution B is 5:1.

[0018] Preferably, when the prepared electrochromic film is a Prussian blue film, solution A is a mixed aqueous solution of ferric chloride and sodium citrate, the concentration of ferric chloride is 0.05-0.5M, more preferably 0.1M, the molar ratio of sodium citrate to ferric chloride is 1:1-10, more preferably 1:8, the concentration of solution B potassium ferrocyanide aqueous solution is 0.01-0.1M, more preferably 0.05M, and the volume ratio of solution A to solution B is 1:1.

[0019] Preferably, when the electrochromic film is a tungsten oxide film, the chemical bath deposition conditions are 50-90°C, 0.5-5h, further 60°C, 50min; when the electrochromic film is a Prussian blue film, the chemical bath deposition conditions are 10-50°C, 0.5-12h, further 25°C, 12h.

[0020] When the electrochromic film is a tungsten oxide film, the annealing process conditions are 300°C-600°C, 1-24h, further 400°C, 2h; when the electrochromic film is a tungsten oxide film, the drying conditions are 25-75°C, 0.1-5h, further 60°C, 1h.

[0021] The present invention also provides an electrochromic film, which is prepared by the method for preparing the large-area, high-performance electrochromic film.

[0022] The present invention also provides a device for preparing the electrochromic film, comprising a reaction tank assembly, a liquid inlet pipe, a bubbling tube, an oven, a hydraulic lifting device and a roller slide device, wherein the reaction tank assembly is used for performing a chemical bath deposition reaction, the liquid inlet pipe is used for conveying a raw material liquid for performing a chemical bath deposition reaction, the bubbling tube is used for conveying a gas into the reaction tank assembly to improve the uniformity of the reaction solution, the reaction tank assembly is located inside the oven, the oven is used for regulating the temperature of the electrochromic film preparation process, the hydraulic lifting device and the roller slide device are used for moving the reaction tank assembly; the device comprises at least two reaction tank assemblies.

[0023] Preferably, part of the bubbling tube extends into the reaction tank assembly, and a vent hole is provided on the bubbling tube extending into the reaction tank assembly. The vent hole diameter is preferably 1.5 mm, so that a stable airflow (air) can be introduced into the reaction tank assembly during the reaction process to improve the uniformity of the solution, which is beneficial to improving the quality uniformity of the electrochromic film.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] (1) The method of the present invention has simple and mild process conditions, a simple reaction device, and low preparation cost. It can realize large-area uniform preparation of tungsten oxide and Prussian blue films and is easy to operate. It has broad prospects in practical industrial applications.

[0026] (2) During the deposition of Prussian blue, the addition of citrate compounds can act as a chelating agent to reduce the nucleation rate of crystals and prevent crystal aggregation, allowing them to grow evenly on the substrate. During the deposition of tungsten oxide film, citrate compounds form complexes with tungsten ions. The chelation of citrate reduces the reaction rate and helps to form a uniform film. In addition, citrate can also induce the formation of tungsten oxide nanosheet morphology films. This morphology provides more reaction sites during the electrochromic process while reducing the diffusion distance of ions, which is beneficial to the electrochromic performance.

[0027] (3) The area of ​​the electrochromic film obtained by the method of the present invention can reach 15 cm*15 cm, and the uniformity is good, and the transmittance curves at different points on the film have a high degree of overlap. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 These are digital photos of the tungsten oxide film and the Prussian blue film prepared in Example 1.

[0029] Figure 2 These are SEM images of the tungsten oxide film and the Prussian blue film prepared in Example 1, wherein A is a cross-sectional morphology of the tungsten oxide film, B is a surface morphology of the tungsten oxide film, C is a cross-sectional morphology of the Prussian blue film, and D is a surface morphology of the Prussian blue film.

[0030] Figure 3 The XRD patterns of the tungsten oxide film and the Prussian blue film prepared in Example 1 are shown.

[0031] Figure 4 The transmittance variation curve at 633 nm of the tungsten oxide film and the Prussian blue film prepared in Example 1 during repeated coloring and fading is shown in FIG.

[0032] Figure 5 The transmittance curves of the tungsten oxide film and the Prussian blue film prepared in Example 1 under different bias voltages.

[0033] Figure 6 A schematic diagram of a device for preparing the electrochromic film.

[0034] Figure 7 This is a digital photo of the large-area tungsten oxide film and the Prussian blue film prepared in Example 1, with the tungsten oxide film on the left and the Prussian blue film on the right.

[0035] Figure 8 The transmittance spectra of different points of the large-area tungsten oxide film and the Prussian blue film prepared in Example 1 are shown.

[0036] Fig. 9This is a diagram showing the coloring and fading effects of an electrochromic device in which the large-area tungsten oxide film and the Prussian blue film prepared in Example 1 are used as the cathode and anode, respectively. DETAILED DESCRIPTION

[0037] The present invention is further illustrated below in conjunction with the examples and accompanying drawings. It should be understood that these examples are only used to illustrate the present invention and are not intended to limit the scope of the present invention. The operating methods in the following examples without specifying specific conditions are usually carried out under conventional conditions or under conditions recommended by the manufacturer.

[0038] Example 1

[0039] The FTO transparent conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water respectively, and dried for later use.

[0040] Preparation of tungsten oxide (WO3) film: prepare a mixed aqueous solution of sodium tungstate and sodium citrate and mark it as solution A1. In solution A1, the concentration of sodium tungstate is 0.03M and the concentration of sodium citrate is 0.06M; prepare 3M hydrochloric acid and mark it as solution B1; place the treated FTO substrate in a reaction chamber, add solution A1 and solution B1 with a volume ratio of 5:1 into the reaction chamber at the same time, and adjust the temperature to 60°C. After 50 minutes, take out the substrate to obtain a tungsten oxide precursor film; anneal the tungsten oxide precursor film at 400°C for 2h to obtain a tungsten oxide film.

[0041] Preparation of Prussian blue (PB) film: a mixed aqueous solution of ferric chloride and sodium citrate is prepared and recorded as solution A2. In solution A2, the concentration of ferric chloride is 0.1M, the concentration of sodium citrate is 0.0125M, and a potassium ferrocyanide aqueous solution with a concentration of 0.05M is prepared and marked as solution B2; the treated FTO substrate is placed in a reaction chamber, and solution A2 and solution B2 with a volume ratio of 1:1 are added to the reaction chamber at the same time, and the temperature is adjusted to 25°C. After 12 hours, the substrate is taken out to obtain a Prussian blue precursor film; the Prussian blue precursor film is dried at 60°C for 1 hour to obtain a Prussian blue film.

[0042] Figure 1 This is a digital photo of the tungsten oxide film and the Prussian blue film prepared in Example 1. It can be seen that the electrochromic film is evenly distributed on the FTO substrate, indicating that uniform WO3 and PB electrochromic films can be prepared by chemical bath deposition.

[0043] The surface and cross-sectional morphologies of the tungsten oxide film and the Prussian blue film prepared in Example 1 were tested using a scanning electron microscope. Figure 2 As shown in AD, tungsten oxide is a flake morphology that grows vertically on the substrate with a thickness of 505nm; Prussian blue is a planar morphology with cracks with a thickness of 346nm.

[0044] The crystal structures of the tungsten oxide film and the Prussian blue film prepared in Example 1 were tested by XRD. The results are as follows: Figure 3 As shown, the crystal structure of tungsten oxide is triclinic phase, while that of Prussian blue is cubic phase.

[0045] The electrochromic properties of the tungsten oxide film and the Prussian blue film prepared in Example 1 were tested in situ by using Shanghai Chenhua CHI660E and Agilent Cary 5000 spectrometer. 0.5MPC-LiClO4 was used as the electrolyte, platinum sheet was used as the counter electrode, and Ag / AgCl was used as the reference electrode. The curve of the transmittance change of the film at 633nm over time during the coloring and fading process was as shown in the figure. Figure 4 As shown in the figure, it can be seen that the coloring / fading time of the tungsten oxide film is 7.6s / 2.8s, and the coloring / fading time of the Prussian blue film is 2.7s / 2.6s, and the response speed is fast; the transmittance under different bias voltages is shown in Figure 5 As shown, it can be seen that the tungsten oxide film exhibits excellent light modulation amplitude in both the visible light band and the near-infrared band (70.8% at 633nm and 71.7% at 1200nm), ensuring the ability of the tungsten oxide film to perform color regulation and photothermal regulation. The regulation of the Prussian blue film mainly occurs in the visible light band, with a maximum light modulation amplitude of 83% at 633nm.

[0046] In addition, through experimental verification, the method in this embodiment can prepare a large-area electrochromic film (15cm*15cm) Figure 7 ), Figure 8 The results show that in the 300-1600nm band, the transmittance curves of the Prussian blue film at different points almost completely overlap, and the transmittance curves of the tungsten oxide film at different points have only a small deviation, indicating that the prepared large-area film has good uniformity.

[0047] The EC energy storage device was prepared by using Prussian blue (PB) film as the cathode electrode and tungsten oxide (WO3) film as the anode electrode, assembling with double-sided tape, injecting 0.5M PC-LiClO4 electrolyte into the gap (1mm) between the PB and WO3 electrodes, and using Cu foil to ensure the connection between the conductive substrate and the external circuit. Finally, the device was wrapped with a seal and welded to ensure good sealing performance. The prepared electrochromic device can work in both colored and faded states. Fig. 9 The left side in the middle is the working state of colorization, with low transmittance, dim colors, and unclear character details. The right side is the working state of fading state, with high overall transmittance, bright colors, and clear character details.

[0048] Example 2

[0049] The FTO transparent conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water respectively, and dried for later use.

[0050] Preparation of tungsten oxide (WO3) film: prepare a mixed aqueous solution of sodium tungstate and citric acid and mark it as solution A1. In solution A1, the concentration of sodium tungstate is 0.03M and the concentration of citric acid is 0.06M; prepare 3M hydrochloric acid and mark it as solution B1; place the treated FTO substrate in the reaction chamber, add solution A1 and solution B1 with a volume ratio of 5:1 into the reaction chamber at the same time, and adjust the temperature to 60℃. After 1h, take out the substrate to obtain a tungsten oxide precursor film; anneal the tungsten oxide precursor film at 400℃ for 1h to obtain a tungsten oxide film.

[0051] Preparation of Prussian blue (PB) film: a mixed aqueous solution of ferric chloride and citric acid is prepared and recorded as solution A2. In solution A2, the concentration of ferric chloride is 0.1M, the concentration of citric acid is 0.0125M, and a potassium ferrocyanide aqueous solution with a concentration of 0.05M is prepared and marked as solution B2; the treated FTO substrate is placed in a reaction chamber, and solution A2 and solution B2 with a volume ratio of 1:1 are added to the reaction chamber at the same time, and the temperature is adjusted to 25°C. After 10 hours, the substrate is taken out to obtain a Prussian blue precursor film; the Prussian blue precursor film is dried at 60°C for 1 hour to obtain a Prussian blue film.

[0052] Example 3

[0053] The FTO transparent conductive glass was ultrasonically cleaned in acetone, anhydrous ethanol and deionized water respectively, and dried for later use.

[0054] Preparation of tungsten oxide (WO3) film: prepare a mixed aqueous solution of sodium tungstate and sodium citrate and mark it as solution A1. In solution A1, the concentration of sodium tungstate is 0.03M and the concentration of sodium citrate is 0.09M; prepare 3M hydrochloric acid and mark it as solution B1; place the FTO substrate treated in the above steps in a reaction chamber, add solution A1 and solution B1 with a volume ratio of 5:1 into the reaction chamber at the same time, and adjust the temperature to 60°C. After 0.5h, take out the substrate to obtain a tungsten oxide precursor film; anneal the tungsten oxide precursor film at 400°C for 1h to obtain a tungsten oxide film.

[0055] Preparation of Prussian blue (PB) film: a mixed aqueous solution of ferric chloride and sodium citrate is prepared and recorded as solution A2. In solution A2, the concentration of ferric chloride is 0.1M, the concentration of sodium citrate is 0.1M, and a potassium ferrocyanide aqueous solution with a concentration of 0.05M is prepared and marked as solution B2; the treated FTO substrate is placed in a reaction chamber, and solution A2 and solution B2 with a volume ratio of 1:1 are added to the reaction chamber at the same time, and the temperature is adjusted to 25°C. After 8 hours, the substrate is taken out to obtain a Prussian blue precursor film; the Prussian blue precursor film is dried at 60°C for 1 hour to obtain a Prussian blue film.

[0056] Comparative Example 1

[0057] In this comparative example, the preparation method of tungsten oxide is different from that of Example 1 only in that sodium citrate is not added, and the other process conditions and parameters are the same; the preparation method of Prussian blue film is different from that of Example 1 only in that sodium citrate is not added, and the other process conditions and parameters are the same.

[0058] The microscopic morphology of the tungsten oxide prepared in this comparative example is micron-block, discontinuous film formation, and no electrochromic performance. The fading time of the Prussian blue film is significantly slower than that of Example 1, and the modulation amplitude is lower than that of Example 1.

[0059] Comparative Example 2

[0060] In this comparative example, the preparation method of the tungsten oxide film is different from that of Example 1 only in that the molar ratio of sodium citrate to sodium tungstate is 4:1, and the other process conditions and parameters are the same; the preparation method of the Prussian blue film is different from that of Example 1 only in that the molar ratio of sodium citrate to ferric chloride is 2:1, and the other process conditions and parameters are the same.

[0061] The tungsten oxide film prepared in this comparative example has dispersed micron-scale petal-like morphology, which will cause serious light scattering and is not conducive to the application of transmission electrochromic devices; the density of the Prussian blue film is lower than that of Example 1, and thus the electrochromic performance is also worse than that of Example 1.

[0062] Example 4

[0063] The embodiment of the present invention also provides a device for preparing the electrochromic film, such as Figure 6As shown, it includes two reaction tank assemblies, a liquid inlet pipe, a bubbling tube, an oven, a hydraulic lifting device and a roller slide device. The reaction tank assembly is used for chemical bath deposition reaction, the liquid inlet pipe is used for conveying raw material liquid for chemical bath deposition reaction, the bubbling tube is used for conveying gas into the reaction tank assembly, part of the bubbling tube extends into the reaction tank assembly, and a vent is arranged on the bubbling tube extending into the reaction tank assembly. The vent aperture is 1.5 mm, so that a stable airflow is blown into the reaction tank during the reaction process to improve the uniformity of the reaction solution, which is beneficial to depositing a film of uniform quality on the substrate. The liquid inlet pipe and the bubbling tube are connected and assembled with the bracket through a polytetrafluoroethylene support. The reaction tank assembly is located inside the oven. The oven is used to regulate the temperature of the process of preparing the electrochromic film. The hydraulic lifting device and the roller slide device are used to move the reaction tank assembly.

[0064] The embodiments described above provide a detailed description of the technical solutions of the present invention. It should be understood that the above are only specific embodiments of the present invention and are not intended to limit the present invention. Any modifications, supplements or similar substitutions made within the scope of the principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a large-area, high-performance electrochromic film, characterized in that: The following steps are involved: (1) preparing a precursor solution required for a chemical bath deposition reaction, wherein the precursor solution includes a solution A and a solution B; (2) placing a transparent conductive substrate in a reaction chamber, adding solution A and solution B at the same time, performing chemical bath deposition to obtain a precursor film, and performing post-treatment on the precursor film to obtain the large-area, high-performance electrochromic film; When the electrochromic film is a tungsten oxide film, solution A is a mixed aqueous solution of tungstate and a citrate-containing compound, solution B is hydrochloric acid, and the post-treatment step is an annealing process; When the prepared electrochromic film is a Prussian blue film, solution A is a mixed aqueous solution of iron salt and a citrate-containing compound, solution B is an aqueous solution of potassium ferrocyanide, and the post-treatment step is a drying process.

2. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: The transparent conductive substrate includes ITO transparent conductive glass, FTO transparent conductive glass, AZO transparent conductive glass, GZO transparent conductive glass or a metal nanowire network transparent electrode.

3. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: When the electrochromic film is a tungsten oxide film, solution A is a mixed aqueous solution of sodium tungstate and sodium citrate or a mixed aqueous solution of sodium tungstate and citric acid; when the electrochromic film is a Prussian blue film, solution A is a mixed aqueous solution of ferric chloride and sodium citrate or a mixed aqueous solution of ferric chloride and citric acid.

4. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: When the prepared electrochromic film is a tungsten oxide film, solution A is a mixed aqueous solution of sodium tungstate and sodium citrate, the concentration of sodium tungstate is 0.01-0.1M, the molar ratio of sodium citrate to sodium tungstate is 1.5-3.5:1, the concentration of hydrochloric acid in solution B is 1-5M, and the volume ratio of solution A to solution B is 5:

1.

5. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: When the prepared electrochromic film is a Prussian blue film, solution A is a mixed aqueous solution of ferric chloride and sodium citrate, the concentration of ferric chloride is 0.05-0.5M, the molar ratio of sodium citrate to ferric chloride is 1:1-10, the concentration of solution B potassium ferrocyanide aqueous solution is 0.01-0.1M, and the volume ratio of solution A to solution B is 1:

1.

6. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: When the electrochromic film is a tungsten oxide film, the chemical bath deposition conditions are 50-90°C, 0.5-5h; when the electrochromic film is a Prussian blue film, the chemical bath deposition conditions are 10-50°C, 0.5-12h.

7. The method for preparing a large-area, high-performance electrochromic film according to claim 1, characterized in that: When the electrochromic film is a tungsten oxide film, the annealing process is carried out at 300-600°C for 1-24 hours; when the electrochromic film is a tungsten oxide film, the drying process is carried out at 25-75°C for 0.1-5 hours.

8. An electrochromic film, characterized in that: The electrochromic film is prepared by the method for preparing a large-area, high-performance electrochromic film according to any one of claims 1 to 7.

9. A device for preparing the electrochromic film according to claim 8, characterized in that: The invention comprises a reaction tank assembly, a liquid inlet pipe, a bubbling tube, an oven, a hydraulic lifting device and a roller slide device. The reaction tank assembly is used for chemical bath deposition reaction. The liquid inlet pipe is used for conveying raw material liquid for chemical bath deposition reaction. The bubbling tube is used for conveying gas into the reaction tank assembly to improve the uniformity of the reaction solution. The reaction tank assembly is located inside the oven. The oven is used for regulating the temperature of the process of preparing the electrochromic film. The hydraulic lifting device and the roller slide device are used for moving the reaction tank assembly. The device comprises at least two reaction tank assemblies.

10. The device according to claim 9, characterized in that A vent hole is arranged on the bubbling tube extending into the reaction tank assembly.

Citation Information

Patent Citations

  • Method for synthesizing tungsten trioxide electrochromic material by one step with assistance of citric acid

    CN107827159A

  • Prussian blue composite material as well as preparation method and application thereof

    CN115505939A

Cited By

  • Preparation method of electrochromic multicolor thin film device

    CN119987091A

  • Porous magnetron sputtering electrochromic film as well as preparation method and application thereof

    CN121046800A