High-temperature durable cementing material synthesized by utilizing lithium slag and method of high-temperature durable cementing material

Through two-step calcination and microwave assisted technology, the problem of utilization of high-content elements of lithium slag was solved, and a high-temperature durable low-alite-high-belitt-sulfaluminate gelling material was prepared, realizing the resource utilization of lithium slag and Environmentally friendly gelling material process, with long-term durability and low-carbon characteristics.

CN118993585APending Publication Date: 2024-11-22JIANGXI BUILDING MATERIALS RES & DESIGN INST CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410997845.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

Due to the high content of sulfur, potassium and sodium, the existing lithium slag cannot be effectively used to prepare silicate cement clinker, and the landfill of lithium slag leads to environmental pollution, and the gelling materials prepared by calcining lithium slag are mechanically employed at high temperatures and long-term. The performance is degraded, limiting its application.

Method used

Using a two-step calcination method, calcium, lithium mica lithium slag, aluminum and iron raw materials are mixed in a specific proportion. After the first and second calcination, microwave-assisted insulation is used during the calcination process to produce low-ali Te-GaoBelite-Calcium Sulfurate gelling material.

Benefits of technology

The lithium slag resource utilization was achieved, and gelled materials with long-term durability and low-carbon characteristics were prepared at high temperatures, which reduced environmental pollution and maintained the later strength growth under the influence of high potassium sodium, reaching 42.5 silicate Performance requirements for salt cement clinker.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118993585A_ABST
    Figure CN118993585A_ABST
Patent Text Reader

Abstract

The invention provides a high-temperature durable cementing material synthesized from lithium slag and a method thereof, and belongs to the technical field of building materials.The method comprises the steps that a calcium raw material, lepidolite lithium slag, an aluminum raw material and an iron raw material are mixed according to a set proportion to prepare a raw material; after pressing into sheets, carrying out first calcination according to a set heating program; quenching to room temperature, and grinding to obtain primary calcined clinker; adding calcium fluoride into the primary calcined clinker, mixing, adding water, ball-milling into powder, pressing into sheets, and performing secondary calcination according to a set heating program to obtain a secondary calcined product; and quenching to room temperature, and grinding to obtain the high-temperature durable low alite-high belite-calcium sulphoaluminate cementing material. The calcium sulphoaluminate cementing material with low alite and high belite is prepared by fully utilizing high-content elements (potassium and sodium) in the lithium slag and adopting a two-step calcination method, and the calcium sulphoaluminate cementing material has long-age durability in a 50 DEG C high-temperature curing environment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of building materials, and particularly relates to a high-temperature durable gelling material synthesized by using lithium slag and a method thereof. Background Art

[0002] Lepidolite is the most common lithium mineral, a basic aluminum silicate of potassium and lithium, and an important mineral for lithium extraction. In daily applications, lithium extraction from lepidolite using the sulfuric acid method produces a large amount of lithium slag, which contains sulfur and high potassium and sodium elements. If the lithium slag is landfilled on site, it will pollute the local soil and water quality.

[0003] In the past, lithium slag was used to replace clay as raw material for firing ordinary Portland cement clinker due to its silicon-alumina characteristics. At that time, lithium slag with extremely low sulfur content was used. However, with the improvement of lithium extraction technology, most lithium slag in actual projects currently has high sulfur, potassium and sodium content, and thus cannot be used to prepare Portland cement clinker, which cannot meet the demand for large-scale consumption of lithium slag.

[0004] In order to solve the above problems, existing studies have mixed lithium slag with iron raw materials and aluminum raw materials and calcined them to obtain high alite-belite-calcium sulfoaluminate cementitious materials, which have good compressive and flexural strength.

[0005] However, studies have found that cement prepared with the cementitious material using the above method has excellent compressive and flexural strength only in the short term (such as 28 days) and at room temperature. As time goes by and the temperature rises, its mechanical properties will decrease, which in turn limits its application and promotion. Summary of the invention

[0006] In view of this, the present invention aims to provide a high-temperature durable gelling material synthesized using lithium slag and a method thereof, aiming to solve at least one technical problem in the background technology.

[0007] The present invention is achieved in that:

[0008] A method for synthesizing a high-temperature durable gelling material using lithium slag, the method comprising the following steps:

[0009] The calcium raw material, lithium mica slag, aluminum raw material and iron raw material are mixed in a set ratio to prepare raw material;

[0010] After the raw material is pressed into sheets, it is calcined for the first time according to a set temperature rising program to obtain a primary calcined product;

[0011] Rapidly cooling the primary calcined product to room temperature, and grinding it to obtain primary calcined clinker;

[0012] Calcium fluoride is added to the primary calcined clinker, mixed, and then water is added and ball-milled into powder, which is pressed into tablets and then calcined for the second time according to a set temperature rise program to obtain a secondary calcined product;

[0013] The secondary calcined product is rapidly cooled to room temperature and ground to obtain a high-temperature durable gelling material, which is a low-alite-high-belite-calcium sulfoaluminate gelling material.

[0014] Further, the first calcination adopts the following operation:

[0015] Heating at a rate of 10-15°C / min to 900-950°C, keeping the temperature for 0.5-1h;

[0016] The temperature is raised to 1200-1240° C. at a heating rate of 10-15° C. / min and kept at that temperature for 1-30 minutes to obtain a primary calcination product.

[0017] Further, the second calcination adopts the following operation:

[0018] Heating at a rate of 10-15°C / min to 900-950°C, keeping the temperature for 0.5-1h;

[0019] The temperature is raised to 1300-1350° C. at a heating rate of 10-15° C. / min and kept at that temperature for 1-30 minutes to obtain a secondary calcination product.

[0020] Furthermore, microwave-assisted heat preservation is used during both the first calcination and the second calcination.

[0021] Furthermore, the calcium raw material, lithium mica slag, aluminum raw material and iron raw material are mixed according to a set ratio to prepare raw material, and the specific operation is as follows:

[0022] After grinding the raw materials to 200-500 mesh respectively, mix them evenly according to the set ratio to obtain a mixed material;

[0023] Add 5-10 wt% of water to the mixture and stir evenly, then perform high-energy ball milling to obtain raw material;

[0024] Among them, the weight ratio of calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material is (50-55): (30-45): (1-10): (1-5).

[0025] Furthermore, the calcium raw material is at least one of limestone, quicklime or slaked lime;

[0026] The aluminum raw material is at least one of aluminum ash, aluminum mud or bauxite;

[0027] The iron raw material is iron-containing nonferrous metal ash, hematite, magnetite or iron tailings.

[0028] Furthermore, the lithium mica slag contains the following components in weight percentage:

[0029] SiO2 20~40%;

[0030] Al2O3 15~25%;

[0031] Fe2O3 1~5%;

[0032] SO3 5~20%;

[0033] CaO 10-30%;

[0034] K2O 1~10%;

[0035] Na2O 1~10%;

[0036] The balance is other impurities.

[0037] Furthermore, the specific surface area of ​​the primary calcined product or the secondary calcined product after grinding is 350 to 500 m 2 / kg.

[0038] Furthermore, the amount of calcium fluoride used is 1-2wt% of the primary calcined clinker.

[0039] The present invention also provides a high-temperature durable gelling material synthesized by the above method, wherein the high-temperature durable gelling material is a low-alite-high-belite-calcium sulfoaluminate gelling material.

[0040] Compared with the prior art, the present invention has the following beneficial effects:

[0041] 1. The present invention makes full use of the high content of elements (potassium and sodium) in lithium slag and adopts a two-step calcination method to prepare a calcium sulphoaluminate cementitious material with low alite and high belite, which has long-term durability under a high temperature (50°C) curing environment.

[0042] 2. The present invention provides a method for resource utilization of lithium mica slag, which provides an effective way to solve the problem of recycling and reusing waste slag after lithium extraction.

[0043] 3. The present invention reduces environmental pollution and has a low calcination temperature. The method has the characteristics of low carbon and is a green cementitious material process method. Although the prepared cementitious material has low initial strength under the influence of high potassium and sodium, its later strength continues to develop and its performance can still reach 42.5 silicate cement clinker performance requirements at high temperatures, and has broad promotion prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0044] Figure 1 This is the XRD diagram of the low alite-high belite-calcium sulfoaluminate cementitious material prepared in Example 1 of the present invention. DETAILED DESCRIPTION

[0045] In order to make the purpose, technical solution and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific implementation cases described herein are only used to explain the present invention and are not used to limit the present invention.

[0046] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0047] S1, mixing a calcium raw material, lithium mica slag, an aluminum raw material and an iron raw material according to a set ratio to prepare a raw material;

[0048] The calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material after drying are ground to 200-500 mesh respectively, and then the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material are mixed in a mixer at a weight ratio of (50-55): (30-45): (1-10): (1-5) for 24 hours to obtain a mixture, and water accounting for 5-10% of the mixture is added to the mixture, and then the mixture is added to a high-energy ball mill, and high-energy ball milling is performed at 200-800 r / min for 15-60 minutes to obtain a raw material;

[0049] Among them, the calcium raw material is at least one of limestone, quicklime or slaked lime; the aluminum raw material is at least one of aluminum ash, aluminum mud or high / medium / low grade bauxite; the iron raw material is iron-containing non-ferrous metal ash slag, hematite, magnetite or iron tailings; the lithium mica slag contains the following weight percentage components: SiO2: 20-40%, Al2O3: 15-25%, Fe2O3: 1-5%, SO3: 5-20%, CaO: 10-30%, K2O: 1-10%, Na2O: 1-10%. Other impurities are 0-10%, and the lithium mica slag is used as a silicon-aluminum-calcium raw material, accompanied by high potassium and sodium content; in the following embodiments, each embodiment uses limestone as a calcium raw material, aluminum mud as an aluminum raw material, and iron-containing non-ferrous metal ash slag as an iron raw material. The chemical composition of the raw materials used is shown in Table 1, but is not limited thereto.

[0050] Table 1 Summary of chemical composition of raw materials / %

[0051]

[0052]

[0053] S2, after the raw material is pressed into sheets, the first calcination is performed according to a set temperature rise program to obtain a primary calcination product;

[0054] After the raw material is pressed into sheets, it is placed in a box-type resistance furnace, first heated to 900-950°C at a heating rate of 10-15°C / min, kept warm for 0.5-1h, then heated to 1200-1240°C at a heating rate of 10-15°C / min, kept warm for 1-30min, to obtain a primary calcined product;

[0055] Microwave-assisted heat preservation is used during calcination, with a microwave frequency of 2.45 GHz and a power of 500-800 W.

[0056] S3, the primary calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground into 350-500m 2 / kg, and obtain once calcined clinker.

[0057] S4, adding calcium fluoride to the primary calcined clinker, adding 5-10wt% of water, adding the mixture to a high-energy ball mill, performing high-energy ball milling at 200-800r / min for 15-60min, pressing into tablets, and performing a second calcination according to a set temperature rise program to obtain a secondary calcination product;

[0058] 1%-2% calcium fluoride is added to the primary calcined clinker, and the mixture is mixed in a mixer for 24 hours to obtain a raw material. The raw material is pressed into sheets, and then placed in a box-type resistance furnace, and the temperature is first increased to 900-950°C at a heating rate of 10-15°C / min, and kept warm for 0.5-1h, and then increased to 1300-1350°C at a heating rate of 10-15°C / min, and kept warm for 1-30min to obtain a secondary calcined product;

[0059] Microwave-assisted heat preservation is used during calcination, with a microwave frequency of 2.45 GHz and a power of 500-800 W.

[0060] S5. Place the secondary calcined product in a cooling furnace for rapid cooling, and grind it to 350-500 mm after cooling to room temperature. 2 / kg, a high temperature durable low alite-high belite-calcium sulfoaluminate cementitious material was obtained.

[0061] Example 1

[0062] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0063] (1) taking dried calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material and grinding them to 200-500 mesh respectively, mixing the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material in a mass ratio of 50:40:5:5, mixing in a mixer for 24 hours to obtain a mixture, adding water accounting for 5% of the mixture to the mixture, adding the mixture to a high-energy ball mill for high-energy ball milling (the rotation speed of the high-energy ball mill is 500 r / min, and the time is 15 minutes) to obtain a raw material;

[0064] (2) After the raw material is pressed into sheets, it is placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 900°C at a heating rate of 10°C / min, and kept at this temperature for 0.5h, and then increased to 1200°C at a heating rate of 15°C / min, and kept at this temperature for 30min with microwave assistance, with a microwave frequency of 2.45GHz and a power of 800W, to obtain a primary calcined product;

[0065] (3) The calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground to obtain a primary calcined clinker.

[0066] (4) The primary calcined clinker is mixed with 2% calcium fluoride, mixed in a mixer for 24 hours to obtain a mixture, 5% water is added to the mixture, and then added to a high-energy ball mill for high-energy ball milling (the speed of the high-energy ball mill is 500 r / min, and the time is 15 min);

[0067] (5) The powder obtained in step (4) is pressed into a sheet, and then placed in a box-type resistance furnace with a microwave function, and the temperature is first increased to 900° C. at a heating rate of 10° C. / min, and kept at this temperature for 0.5 h, and then increased to 1330° C. at a heating rate of 15° C. / min, and kept at this temperature for 30 min with microwave assistance, with a microwave frequency of 2.45 GHz and a power of 800 W, to obtain a secondary calcined product;

[0068] (6) placing the secondary calcined product in a cooling furnace for rapid cooling, cooling to room temperature, and then grinding to obtain a low-alite-high-belite-calcium sulfoaluminate cementitious material.

[0069] The XRD pattern of the low alite-high belite-calcium sulphoaluminate cementitious material prepared in Example 1 is shown in Figure 1 It can be seen that the low alite-high belite-calcium sulfoaluminate cementitious material is mainly composed of C2S, C4A3$, C4AF and C3S. According to quantitative analysis, the clinker contains 52.65% C2S, 25.49% C4A3S, 12.38% C4AF, 5.13% C3S and 4.2% other minerals.

[0070] Example 2

[0071] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0072] (1) taking the dried calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material and grinding them to 200-500 mesh respectively, mixing the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material in a mass ratio of 55:35:2:8, mixing in a mixer for 24 hours to obtain a mixture, adding water accounting for 5% of the mixture to the mixture, adding the mixture to a high-energy ball mill for high-energy ball milling (the rotation speed of the high-energy ball mill is 500 r / min, and the time is 15 minutes) to obtain a raw material;

[0073] (2) After the raw material is pressed into sheets, it is placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 950°C at a heating rate of 15°C / min, and then heated to 1240°C at a heating rate of 15°C / min, and microwave-assisted heating is performed for 20 minutes. The microwave frequency is 2.45 GHz and the power is 800 W to obtain a primary calcined product;

[0074] (3) The calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground to obtain a primary calcined clinker.

[0075] (4) 1% calcium fluoride was added to the primary calcined clinker, and the mixture was mixed in a mixer for 24 hours to obtain a mixture. After 5% water was added to the mixture, the mixture was added to a high-energy ball mill for high-energy ball milling (the speed of the high-energy ball mill was 500 r / min, and the time was 15 min);

[0076] (5) The powder obtained in step (4) is pressed into tablets, and then placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 900° C. at a heating rate of 15° C. / min, and kept warm for 1 hour, and then increased to 1350° C. at a heating rate of 15° C. / min, and kept warm for 20 minutes with microwave assistance, with a microwave frequency of 2.45 GHz and a power of 800 W, to obtain a secondary calcined product;

[0077] (6) placing the secondary calcined product in a cooling furnace for rapid cooling, cooling to room temperature, and then grinding to obtain a low-alite-high-belite-calcium sulfoaluminate cementitious material.

[0078] Example 3

[0079] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0080] (1) taking the dried calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material and grinding them to 200-500 mesh respectively, mixing the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material in a mass ratio of 52:43:1:4, mixing in a mixer for 24 hours to obtain a mixture, adding water accounting for 5% of the mixture to the mixture, adding the mixture to a high-energy ball mill for high-energy ball milling (the rotation speed of the high-energy ball mill is 500 r / min, and the time is 15 minutes) to obtain a raw material;

[0081] (2) After the raw material is pressed into sheets, it is placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 920°C at a heating rate of 12°C / min, and kept at this temperature for 0.8h, and then increased to 1220°C at a heating rate of 10°C / min, and kept at this temperature for 15min with microwave assistance, with a microwave frequency of 2.45GHz and a power of 500W, to obtain a primary calcined product;

[0082] (3) The primary calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground to obtain primary calcined clinker.

[0083] (4) 1% calcium fluoride was added to the primary calcined clinker, and the mixture was mixed in a mixer for 24 hours to obtain a mixture. After 5% water was added to the mixture, the mixture was added to a high-energy ball mill for high-energy ball milling (the speed of the high-energy ball mill was 500 r / min, and the time was 15 min);

[0084] (5) The powder obtained in step (4) is pressed into tablets, and then placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 900° C. at a heating rate of 10° C. / min, and kept warm for 0.5 h, and then increased to 1320° C. at a heating rate of 15° C. / min, and kept warm for 30 min with microwave assistance, with a microwave frequency of 2.45 GHz and a power of 500 W, to obtain a secondary calcined product;

[0085] (6) placing the secondary calcined product in a cooling furnace for rapid cooling, cooling to room temperature, and then grinding to obtain a low-alite-high-belite-calcium sulfoaluminate cementitious material.

[0086] Example 4

[0087] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0088] (1) taking the dried calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material and grinding them to 200-500 mesh respectively, mixing the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material in a mass ratio of 54:35:4:7, mixing in a mixer for 24 hours to obtain a mixture, adding water accounting for 5% of the mixture to the mixture, adding the mixture to a high-energy ball mill for high-energy ball milling (the rotation speed of the high-energy ball mill is 500 r / min, and the time is 15 minutes) to obtain a raw material;

[0089] (2) After the raw material is pressed into sheets, it is placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 940°C at a heating rate of 10°C / min, and then kept at this temperature for 0.5h, and then increased to 1235°C at a heating rate of 10°C / min, and kept at this temperature for 100min with microwave assistance, with a microwave frequency of 2.45GHz and a power of 800W, to obtain a primary calcined product;

[0090] (3) The primary calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground to obtain primary calcined clinker.

[0091] (4) The primary calcined clinker is mixed with 2% calcium fluoride, mixed in a mixer for 24 hours to obtain a mixture, 5% water is added to the mixture, and then added to a high-energy ball mill for high-energy ball milling (the speed of the high-energy ball mill is 500 r / min, and the time is 15 min);

[0092] (5) the powder obtained in step (4) is pressed into tablets, and then placed in a box-type resistance furnace with microwave function, and the temperature is first increased to 940° C. at a heating rate of 10° C. / min, and kept warm for 0.5 h, and then increased to 1350° C. at a heating rate of 15° C. / min, and kept warm for 30 min with microwave assistance, with a microwave frequency of 2.45 GHz and a power of 800 W, to obtain a secondary calcined product;

[0093] (6) placing the secondary calcined product in a cooling furnace for rapid cooling, cooling to room temperature, and then grinding to obtain a low-alite-high-belite-calcium sulfoaluminate cementitious material.

[0094] Example 5

[0095] A method for synthesizing a high-temperature durable gelling material using lithium slag comprises the following steps:

[0096] (1) taking the dried calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material and grinding them to 200-500 mesh respectively, mixing the calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material in a mass ratio of 51:38:7:4, mixing in a mixer for 24 hours to obtain a mixture, adding water accounting for 5% of the mixture to the mixture, adding the mixture to a high-energy ball mill for high-energy ball milling (the rotation speed of the high-energy ball mill is 500 r / min, and the time is 15 minutes) to obtain a raw material;

[0097] (2) After the raw material is pressed into sheets, it is placed in a box-type resistance furnace with microwave function, firstly heated to 910°C at a heating rate of 12°C / min, kept warm for 0.6h, and then heated to 1210°C at a heating rate of 15°C / min, kept warm for 30min with microwave assistance, microwave frequency of 2.45GHz, power of 700W, to obtain a primary calcined product;

[0098] (3) The primary calcined product is placed in a cooling furnace for rapid cooling, and after cooling to room temperature, it is ground to obtain primary calcined clinker.

[0099] (4) 1.5% calcium fluoride was added to the primary calcined clinker, and the mixture was mixed in a mixer for 24 hours to obtain a mixture. After 5% water was added to the mixture, the mixture was added to a high-energy ball mill for high-energy ball milling (the speed of the high-energy ball mill was 500 r / min, and the time was 15 min);

[0100] (5) The powder obtained in step (4) is pressed into a sheet, and then placed in a box-type resistance furnace with a microwave function, and the temperature is first increased to 910° C. at a heating rate of 10° C. / min, and kept warm for 1 hour, and then increased to 1310° C. at a heating rate of 15° C. / min, and kept warm for 30 minutes with microwave assistance, with a microwave frequency of 2.45 GHz and a power of 800 W, to obtain a secondary calcined product;

[0101] (6) placing the secondary calcined product in a cooling furnace for rapid cooling, cooling to room temperature, and then grinding to obtain a low-alite-high-belite-calcium sulfoaluminate cementitious material.

[0102] Comparative Example 1

[0103] The method for preparing the cementitious material in this comparative example 1 is different from that in Example 1 in that it only includes steps (1) to (3) of Example 1, that is, the cementitious material is prepared by a one-time calcination method.

[0104] The components and properties of the cementitious materials prepared in various embodiments and comparative examples were tested, and the results are shown in Table 2 and Table 3, respectively.

[0105] Table 2

[0106]

[0107]

[0108] It can be seen from Table 2 above that the calcium sulfoaluminate cementitious material prepared by secondary calcination in the embodiment of the present invention achieves the coexistence of alite (C3S) mineral phase and calcium sulfoaluminate mineral phase; while the calcium sulfoaluminate cementitious material prepared by single calcination in Comparative Example 1 has a high calcium sulfoaluminate content but no alite mineral phase, and less ferroaluminite phase (C4AF).

[0109] Performance testing method:

[0110] 15% of dihydrate gypsum was added to the cement clinker obtained in Examples 1 to 5 and Comparative Example 1, respectively. After grinding, the compressive strength and flexural strength of 1d, 28d, and 90d were tested respectively in a high temperature environment of 50°C. The test method was carried out according to GB / T17671-2021 cement mortar strength test method (ISO method), and the test results are shown in Table 3.

[0111] Table 3

[0112]

[0113] It can be seen from Table 3 above that the low alite-high belite-calcium sulfoaluminate cementitious material prepared in the embodiment of the present invention has long-term durability under a high temperature (50°C) curing environment. Although the cementitious material has a low initial strength under the influence of high potassium and sodium, the later strength continues to develop and the performance can still reach the 42.5 silicate cement clinker performance requirements at high temperatures. Although the calcium sulfoaluminate cementitious material prepared in Comparative Example 1 has a high initial strength, its compressive strength and flexural strength are reduced over time; the reason is that the calcium sulfoaluminate cementitious material prepared in Comparative Example 1 has no alite mineral phase at high temperature, and the calcium sulfoaluminate mineral phase is hydrated. The calcium sulfoaluminate generated by the hydration of the calcium sulfoaluminate mineral phase is easy to expand in a high temperature environment, destroying the internal structure of the cement. The early hydration of the alite phase to form CSH gel can still use its own adhesion to form a dense network structure with calcium sulfoxide at high temperature, making the cement almost unaffected at high temperature. At the same time, more ferroaluminite phase (C4AF) can also be hydrated to produce more CAH phase, which also has a positive effect on the high temperature tolerance of cement.

[0114] The above-mentioned embodiments only express several implementation methods of the present invention, and the description thereof is relatively specific and detailed, but it cannot be understood as limiting the scope of the patent of the present invention. It should be pointed out that, for ordinary technicians in this field, several variations and improvements can be made without departing from the concept of the present invention, which all belong to the protection scope of the present invention. Therefore, the protection scope of the patent of the present invention shall be subject to the attached claims.

Claims

1. A method for synthesizing a high-temperature durable gelling material using lithium slag, characterized in that: The method comprises the following steps: The calcium raw material, lithium mica slag, aluminum raw material and iron raw material are mixed in a set ratio to prepare raw material; After the raw material is pressed into sheets, it is calcined for the first time according to a set temperature rising program to obtain a primary calcined product; Rapidly cooling the primary calcined product to room temperature, and grinding it to obtain primary calcined clinker; Calcium fluoride is added to the primary calcined clinker, mixed, and then water is added and ball-milled into powder, which is pressed into tablets and then calcined for the second time according to a set temperature rise program to obtain a secondary calcined product; The secondary calcined product is rapidly cooled to room temperature and ground to obtain a high-temperature durable gelling material; the high-temperature durable gelling material is a low-alite-high-belite-calcium sulfoaluminate gelling material.

2. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: The first calcination is performed as follows: Heating at a rate of 10-15°C / min to 900-950°C, keeping the temperature for 0.5-1h; The temperature is raised to 1200-1240° C. at a heating rate of 10-15° C. / min and kept at that temperature for 1-30 minutes to obtain a primary calcination product.

3. A method for synthesizing high temperature durable gelling material using lithium slag according to claim 1 or 2, characterized in that: The second calcination is carried out as follows: Heating at a rate of 10-15°C / min to 900-950°C, keeping the temperature for 0.5-1h; The temperature is raised to 1300-1350° C. at a heating rate of 10-15° C. / min and kept at that temperature for 1-30 minutes to obtain a secondary calcination product.

4. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: Microwave-assisted heat preservation is adopted during the first calcination and the second calcination.

5. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: The calcium raw material, lithium mica slag, aluminum raw material and iron raw material are mixed in a set ratio to prepare raw material. The specific operation is as follows: After grinding the raw materials to 200-500 mesh respectively, mix them evenly according to the set ratio to obtain a mixed material; Add 5-10 wt% of water to the mixture and stir evenly, then perform high-energy ball milling to obtain raw material; Among them, the weight ratio of calcium raw material, lithium mica lithium slag, aluminum raw material and iron raw material is (50-55): (30-45): (1-10): (1-5).

6. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: The calcium raw material is at least one of limestone, quicklime or slaked lime; The aluminum raw material is at least one of aluminum ash, aluminum mud or bauxite; The iron raw material is iron-containing nonferrous metal ash, hematite, magnetite or iron tailings.

7. A method for synthesizing high temperature durable gelling material using lithium slag according to claim 1 or 6, characterized in that: The lithium mica slag comprises the following components in weight percentage: SiO2 20~40%; Al2O3 15~25%; Fe2O3 1~5%; SO3 5~20%; CaO 10-30%; K2O 1~10%; Na2O 1~10%; The balance is other impurities.

8. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: The specific surface area of ​​the first calcined product or the second calcined product after grinding is 350 to 500 m 2 / kg.

9. The method for synthesizing high temperature durable gelling material using lithium slag according to claim 1, characterized in that: The amount of calcium fluoride used is 1-2 wt% of the primary calcined clinker.

10. A high temperature durable gelling material synthesized by using lithium slag, characterized in that: The method is synthesized by any one of claims 1 to 9.