Organic silicon slag and magnesium slag composite reinforced recycled aggregate and preparation method thereof

Through the compounding of silicone slag and magnesium slag, the preparation method of regenerated aggregates is enhanced, and the alcohol amine aid and grinding process is used to solve the problem of insufficient performance of existing regenerated aggregates, improving water absorption, crushing index and resistance The compressive strength realizes the comprehensive utilization and environmental protection of solid waste.

CN118993604AActive Publication Date: 2024-11-22HENAN UNIV OF SCI & TECH +1
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202411115125.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22
Estimated Expiration
2044-08-14

AI Technical Summary

Technical Problem

The surface of the existing recycled aggregate is rough, has many edges and corners, loose and porous micromorphology, resulting in large water absorption and small crushing indicators, which limits its application range in recycled concrete, and the composite enhancement technology of silicone slag and magnesium slag No related reports.

Method used

The preparation method of regenerated aggregates is enhanced by combining silicone slag and magnesium slag. The reaction activity of the powder is improved through wet grinding and dry grinding processes, and surface modification is used to generate CSH gels and silicate minerals. Fill in microcracks and enhance aggregate performance.

Benefits of technology

The water absorption rate, crushing index and compressive strength of recycled aggregates are improved, making their performance close to natural limestone, expanding the scope of application, realizing the comprehensive utilization of solid waste, and reducing environmental pollution.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention belongs to the field of comprehensive recycling of solid wastes, and particularly relates to organic silicon slag and magnesium slag composite reinforced recycled aggregate and a preparation method thereof. The preparation method comprises the following steps: S1, mixing organic silicon slag, water and an alcohol amine grinding aid, and performing wet grinding to obtain organic silicon slag slurry; s2, magnesium slag and an alcohol amine grinding aid are mixed and subjected to dry grinding, and magnesium slag micro powder is obtained; s3, uniformly mixing the magnesium slag micro powder, the organic silicon slag slurry and water to obtain turbid liquid; s4, the recycled aggregate is soaked in water, surface impurities are removed through ultrasonic cleaning, then the recycled aggregate is taken out and soaked in the turbid liquid obtained in the step S3, stirring is conducted for 24-48 h at the speed of 100-300 r / h, natural drying is conducted after soaking is completed, and the organic silicon slag and magnesium slag composite reinforced recycled aggregate is obtained. According to the invention, comprehensive application of three solid wastes is realized, pollution of solid wastes to environments such as land, air and the like is reduced, a technical path for enhancing the recycled aggregate is provided, and good economic and social benefits are achieved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of comprehensive recycling of solid wastes, and specifically relates to an organic silicon slag and magnesium slag composite reinforced recycled aggregate and a preparation method thereof. Background Art

[0002] Organosilicon materials such as organochlorosilane monomers and their derivatives are increasingly used in various production links in modern industry due to their excellent insulation, waterproof, high temperature resistance and other properties. The global output of organosilicon continues to rise, and my country, as a major producer of organosilicon, accounts for about 67% of the global production capacity. According to statistics, my country's annual output of organosilicon in recent years is about 5 million tons, and about 50,000 tons of waste slurry are also produced each year. After the waste slurry is treated by hydrolysis and other processes, the organosilicon, precious metals and other components are recovered, and the remaining organosilicon slag is mainly composed of silicon powder with large specific surface area and small average particle size, and the rest is a small amount of organosilicon and metal. On the other hand, my country is also the country with the largest production of magnesium metal in the world, and the main smelting process is the Pijiang process. The smelting of magnesium metal by this method will be accompanied by a large amount of magnesium slag. On average, about 6 tons of magnesium slag will be discharged for every ton of crude magnesium produced. If it cannot be properly handled, it will not only pollute the environment, but also cause waste of resources.

[0003] Solid waste from construction waste is often used to produce recycled aggregates. However, since its main components are concrete, sintered bricks, etc., after being made into recycled aggregates, its surface is rough, angular, and its microscopic morphology is mostly loose and porous, which makes its water absorption rate large and its crushing index small, greatly limiting its application scope in recycled concrete. To solve this problem, researchers have developed a variety of methods to enhance recycled aggregates, which can be roughly divided into physical enhancement, chemical modification, composite enhancement, etc., and have achieved many research results. However, there has been no relevant report on the technical route of composite enhanced recycled aggregates using the characteristics of organosilicon slag and magnesium slag. The present invention provides a composite reinforced recycled aggregate of organosilicon slag and magnesium slag and a preparation method thereof, which has good ecological value and economic benefits. Summary of the invention

[0004] In view of the problems and shortcomings of the prior art, the present invention provides an organosilicon slag and magnesium slag composite reinforced recycled aggregate and a preparation method thereof.

[0005] Based on the above purpose, the present invention adopts the following technical solution:

[0006] In a first aspect, the present invention provides a method for preparing a composite reinforced recycled aggregate of organic silicon slag and magnesium slag, comprising the following steps:

[0007] S1: mixing and wet-grinding the organosilicon slag, water and an alcoholamine grinding aid to obtain an organosilicon slag slurry;

[0008] S2: Dry-grinding the magnesium slag and the alcoholamine grinding aid to obtain magnesium slag powder;

[0009] S3: Mixing magnesium slag powder, organosilicon slag slurry and water evenly to obtain a suspension;

[0010] S4: soaking the recycled aggregate in water, ultrasonically cleaning to remove surface impurities, then taking out and soaking in the suspension obtained in step S3, stirring at 100-300r / h for 24-48h, and drying naturally after soaking to obtain a composite reinforced recycled aggregate of organic silicon slag and magnesium slag.

[0011] Preferably, the alcoholamine grinding aid is at least one of triethanolamine, triisopropanolamine, and diethanol monoisopropanolamine.

[0012] Preferably, the water is deionized water.

[0013] Preferably, the weight ratio of water to organosilicon slag in step S1 is (0.45-0.60):1, and the amount of alcoholamine grinding aid used is 0.5%-1.0% of the mass of the organosilicon slag.

[0014] Preferably, the amount of the alcoholamine grinding aid in step S2 is 0.5% to 2% of the mass of the magnesium slag.

[0015] Preferably, the weight ratio of the magnesium slag powder, the organosilicon slag slurry and the water in step S3 is 1:(3-5):(60-80).

[0016] Preferably, the mass fraction of silicon dioxide in the organic silicon slag in step S1 is not less than 99%.

[0017] Preferably, the magnesium slag in step S2 is granular reduced slag produced by the Pidgeon process for magnesium smelting.

[0018] Preferably, the wet grinding time in step S1 is 1 to 2 hours, and the wet grinding is performed until the average particle size of the organosilicon slag is 50 to 100 nm. Furthermore, the wet grinding is performed using a wet ball mill.

[0019] Preferably, the dry grinding time in step S2 is 30 to 60 minutes, and the magnesium slag is dry ground to an average particle size of 10 to 20 μm. Furthermore, the dry grinding is performed using a high-energy ball mill.

[0020] Preferably, the ultrasonic frequency in step S4 is 20 to 100 kHz, and the time is 10 to 20 minutes.

[0021] In a second aspect, the present invention provides a composite reinforced recycled aggregate of organic silicon slag and magnesium slag prepared by the preparation method described in the first aspect.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] 1. The organic impurities in the organosilicon slag used in the present invention are generally organosilane monomers, etc., which have good compatibility with alcoholamine grinding aids, can play the effect of surface modifiers, play a grinding aid role in the ball milling process, and improve grinding efficiency. The main component in the organosilicon slag is silicon powder, i.e. silicon dioxide, which is ground to nanometer particle size under the action of alcoholamine grinding aids. On the one hand, it can react with Ca (OH) 2 produced by hydrolysis of magnesium slag micropowder to generate CSH gel, which is precipitated to the surface of recycled aggregate; on the other hand, nano silicon powder particles have very high reactivity, can enter the microcracks of recycled aggregate and react with the alkaline substances therein, produce silicate gel to fill the cracks, and at the same time, the alkalinity of the microcrack environment is continuously improved, which also promotes the depolymerization-polycondensation reaction of nano silicon powder, and further enhances the recycled aggregate.

[0024] 2. The main mineral components of the magnesium slag powder used in the present invention are: γ-C2S, β-C2S, MgO and f-CaO, which are easy to react in water environment to form CSH gel and precipitate Ca 2+ Mg 2+ , Fe 3+ , OH- plasma, among which Ca 2+ OH - Can react with nano-silicon dioxide to produce silicate minerals; Mg 2+ , Fe 3+ It can react with OH- to generate water-insoluble Mg(OH)2 and Fe(OH)3. In a water environment, the alcohol amine grinding aids and the organosilane impurities in the organosilicon slag can, on the one hand, absorb the insoluble CSH gel, Mg(OH)2, Fe(OH)3, metal cations and other products precipitated from the reaction of nano-silicon powder and magnesium slag powder, and on the other hand, can be adsorbed in the micro-cracks of the recycled aggregate, playing a "bridging" role between the two.

[0025] 3. The present invention makes full use of organosilicon slag as a silicon source and magnesium slag as a calcium source, and utilizes wet grinding and dry grinding processes respectively to improve their reaction activity, thereby providing reaction raw materials for filling microcracks in recycled aggregates, giving full play to the resource properties of organosilicon slag and magnesium slag, and realizing the comprehensive application of three types of solid waste including construction waste solid waste, thereby reducing the pollution of solid waste to the land, air and other environments, providing a technical path to enhance recycled aggregates, and having good economic and social benefits. DETAILED DESCRIPTION

[0026] In order to make the purpose, technical solution and advantages of the present invention clearer and more specific, the present invention is further described in detail by examples below. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] Example 1

[0028] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, the preparation method of which has the following specific steps:

[0029] S1: adding organosilicon slag (silicon dioxide mass fraction not less than 99%), deionized water, and triethanolamine grinding aid into a wet ball mill, wherein the weight ratio of deionized water to organosilicon slag is 0.55:1, and the amount of triethanolamine grinding aid is 0.7% of the weight of the organosilicon slag, and wet grinding for 1.5 hours until the average particle size of the organosilicon slag is 50-100 nm, to obtain organosilicon slag slurry;

[0030] S2: adding magnesium slag and triethanolamine grinding aid into a high-energy ball mill, wherein the amount of triethanolamine grinding aid is 1.2% of the weight of the magnesium slag, and dry grinding for 45 minutes until the average particle size of the magnesium slag is 10-20 μm, to obtain magnesium slag powder;

[0031] S3: Mix magnesium slag powder, organosilicon slag slurry and deionized water in a weight ratio of 1:4:70 to obtain a suspension;

[0032] S4: Soak the recycled aggregate in water, perform ultrasonic treatment at 50kHz for 15 minutes to remove loose particles, sand, organic compounds and other impurities on the surface, then take out and soak in the suspension obtained in step S3, stir at 200r / h for 36 hours, and dry naturally after soaking to obtain a composite reinforced recycled aggregate of organosilicon slag and magnesium slag.

[0033] (I) Investigating the influence of grinding aid types on recycled aggregate

[0034] 1. Sample Preparation

[0035] Example 2

[0036] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those of Example 1, except that the alcohol amine grinding aid added in steps S1 and S2 is triisopropanolamine grinding aid.

[0037] Example 3

[0038] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those of Example 1, except that the alcohol amine grinding aid added in steps S1 and S2 is diethanol monoisopropanolamine grinding aid.

[0039] Comparative Example 1

[0040] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those of Example 1, except that no grinding aid is added in steps S1 and S2.

[0041] 2. Performance test:

[0042] The samples obtained in Examples 1 to 3 and Comparative Example 1 were tested for their water absorption and crushing index according to the method described in GB / T 14685-2022 "Pebble and crushed stone for construction".

[0043] The above samples were prepared into C30 concrete specimens, and the basic mix ratio of the C30 concrete specimens was: 285 kg of P.O42.5 cement, 704 kg of quartz sand with a fineness modulus of 2.2, 1200 kg of continuous graded aggregate, 111 kg of municipal water, and 1% of the mass of cement of a polycarboxylate water reducer with a solid content of 30% per cubic meter of concrete. Then, the 28d compressive strength of the concrete specimens was tested according to the method described in GB / T 50081-2019 "Standard for Test Methods for Mechanical Properties of Ordinary Concrete".

[0044] The test results are shown in Table 1.

[0045] Table 1 Performance test of Examples 1 to 3 and Comparative Example 1

[0046] Performance Indicators Water absorption / % Crushing index / % Compressive strength / MPa Example 1 0.9 10 39.1 Example 2 1.1 10 38.7 Example 3 1 11 39 Comparative Example 1 4.5 13 34.6

[0047] It can be seen from Table 1 that under the same addition conditions, different types of grinding aids have little effect on the performance of recycled aggregates. Among them, the recycled aggregate water absorption rate and crushing index obtained in Example 1 using triethanolamine as a grinding aid are the smallest, and the concrete compressive strength reaches the maximum.

[0048] When no grinding aid is used in Comparative Example 1, the water absorption rate and crushing index of the recycled aggregate increase, and the compressive strength decreases, that is, its various properties decrease significantly.

[0049] (II) Investigating the influence of organic silicon slag slurry ratio on recycled aggregate

[0050] 1. Sample Preparation

[0051] Example 4

[0052] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those in Example 1, except that in step S1, the weight ratio of deionized water to organic silicon slag mud is 0.45:1.

[0053] Example 5

[0054] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those in Example 1, except that in step S1, the weight ratio of deionized water to organic silicon slag mud is 0.60:1.

[0055] Comparative Example 2

[0056] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those of Example 1, except that in step S1, the weight ratio of deionized water to organic silicon slag mud is 0.40:1.

[0057] 2. Performance test:

[0058] The samples obtained in Examples 4 to 5 and Comparative Example 2 were tested for their water absorption and crushing index according to the method described in GB / T 14685-2022 "Pebble and crushed stone for construction".

[0059] The above samples were prepared into C30 concrete specimens, and the basic mix ratio of the C30 concrete specimens was the same as above. Then, the 28d compressive strength of the concrete specimens was tested according to the method described in GB / T 50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".

[0060] The test results are shown in Table 2.

[0061] Table 2 Performance test of Examples 1, 4-5 and Comparative Example 2

[0062] Performance Indicators Water absorption / % Crushing index / % Compressive strength / MPa Example 1 0.9 10 39.1 Example 4 1 11 39.2 Example 5 1.1 12 38.3 Comparative Example 2 1.1 11 39.0

[0063] As shown in Table 2, the indicators of Examples 1, 4 and 5 are relatively close, among which the compressive strength of Example 4 is the highest, 39.2 MPa. The compressive strength of Example 5 is the lowest, 38.3 MPa. This is because different concentrations of organosilicon slag slurry have different reinforcing effects on recycled aggregate.

[0064] In comparative example 2, the water absorption rate of the recycled aggregate is 1.1%, the crushing index is 11, and the compressive strength is 39.0, which is close to the respective embodiments. This indicates that further increasing the concentration of the organic silicon slag slurry has no obvious effect on the strengthening of the recycled aggregate, but is likely to cause a waste of resources.

[0065] (III) Investigating the influence of the ratio of magnesium slag powder, organosilicon slag slurry and deionized water on recycled aggregate

[0066] 1. Sample Preparation

[0067] Example 6

[0068] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those in Example 1, except that in step S3, magnesium slag powder, organic silicon slag slurry and deionized water are mixed in a weight ratio of 1:3:60.

[0069] Example 7

[0070] A composite reinforced recycled aggregate of organosilicon slag and magnesium slag, whose components and preparation method are basically the same as those in Example 1, except that in step S3, magnesium slag powder, organosilicon slag slurry and deionized water are mixed in a weight ratio of 1:3:80.

[0071] Comparative Example 3

[0072] A composite reinforced recycled aggregate of organic silicon slag and magnesium slag, whose components and preparation method are basically the same as those in Example 1, except that in step S3, magnesium slag powder, organic silicon slag slurry and deionized water are mixed in a weight ratio of 1:6:50.

[0073] 2. Performance test:

[0074] The samples obtained in Examples 6 to 7 and Comparative Example 3 were tested for their water absorption and crushing index according to the method described in GB / T 14685-2022 "Pebble and crushed stone for construction".

[0075] The above samples were prepared into C30 concrete specimens, and the basic mix ratio of the C30 concrete specimens was the same as above. Then, the 28d compressive strength of the concrete specimens was tested according to the method described in GB / T 50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".

[0076] The test results are shown in Table 3.

[0077] Table 3 Performance test of Examples 1, 6-7 and Comparative Example 3

[0078] Performance Indicators Water absorption / % Crushing index / % Compressive strength / MPa Example 1 0.9 10 39.1 Example 4 0.9 11 38.6 Example 5 1 10 38.8 Comparative Example 2 1.2 13 35.4

[0079] As shown in Table 3, the ratio of magnesium slag powder, organosilicon slag slurry and deionized water has a significant effect on the reinforcing effect of recycled aggregate. Among them, the performance of Example 1 is better, the crushing index of Example 6 is too large and the compressive strength is too small; the water absorption rate of Example 7 is too large and the compressive strength is too small. However, the deviation of the three data is not large.

[0080] In comparative example 3, magnesium slag powder, organosilicon slag slurry and deionized water were mixed at a weight ratio of 1:6:50, and then the recycled aggregate was treated. The water absorption rate and crushing index details were too large, and the compressive strength details were too small. This shows that high concentrations of magnesium slag powder and organosilicon slag mixed slurry will have a counter-effect on the reinforcing effect of the recycled aggregate.

[0081] (IV) Investigating the influence of organic silicon slag treatment process on recycled aggregate

[0082] 1. Sample Preparation

[0083] Comparative Example 4

[0084] A composite reinforced recycled aggregate of organosilicon slag and magnesium slag, whose components and preparation method are basically the same as those of Example 1, except that the organosilicon slag in step S1 is replaced by pretreated organosilicon slag, and the pretreatment method is: adding the organosilicon slag to an ethanol solution with a concentration of 75%, dissolving, centrifuging, washing with water, and centrifuging again until the mass fraction of organosilane impurities in the organosilicon slag is less than 0.1%.

[0085] Comparative Example 5

[0086] A quartz sand and magnesium slag composite reinforced recycled aggregate, whose components and preparation method are basically the same as those in Example 1, except that the organosilicon slag in step S1 is replaced by a mixture of quartz sand and methyl silicone oil, wherein the mass fraction of silicon dioxide in the quartz sand is not less than 99%, and the amount of methyl silicone oil is 1% of the weight of the quartz sand.

[0087] Comparative Example 6

[0088] A quartz sand and magnesium slag composite reinforced recycled aggregate, whose components and preparation method are basically the same as those in Example 1, except that the organosilicon slag in step S1 is replaced by quartz sand, and the mass fraction of silicon dioxide in the quartz sand is not less than 99%.

[0089] 2. Performance test:

[0090] The samples obtained in Comparative Examples 4 to 6 were tested for their water absorption and crushing index according to the method described in GB / T 14685-2022 "Pebble and crushed stone for construction".

[0091] The above samples were prepared into C30 concrete specimens, and the basic mix ratio of the C30 concrete specimens was the same as above. Then, the 28d compressive strength of the concrete specimens was tested according to the method described in GB / T 50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".

[0092] The test results are shown in Table 4.

[0093] Table 4 Performance test of Example 1 and Comparative Examples 4 to 6

[0094] Performance Indicators Water absorption / % Crushing index / % Compressive strength / MPa Example 1 0.9 10 39.1 Comparative Example 4 1.3 12 34.3 Comparative Example 5 0.8 7 40.4 Comparative Example 6 1.2 13 35.6

[0095] As can be seen from Table 4, the performance indicators of Example 1 and Comparative Example 5 are similar, with water absorption rates of 0.9% and 0.8% respectively, and crushing indicators of 10 and 7 respectively, which can all meet the Class I standard in GB / T 14685-2022 "Pebbles and Crushed Stones for Construction"; when used for C30 concrete, the 28d compressive strengths are 39.1MPa and 40.4MPa respectively. The various indicators in Example 1 are slightly smaller than those in Comparative Example 5. This is because, on the one hand, the purity of silica in quartz sand is higher, and on the other hand, compared with the organosilane impurities in organosilicon slag, methyl silicone oil has better wettability with the interface of recycled aggregate, and can better play the bridging role of surfactant. However, it is worth noting that the high-purity quartz sand and methyl silicone oil used in Comparative Example 5 are relatively expensive, and the feasibility of applying them to the strengthening of recycled aggregate is insufficient.

[0096] Comparative Examples 4 and 6 respectively use treated organosilicon slag and quartz sand to strengthen the recycled aggregate, and try to eliminate the influence of organosilane impurities. The performance indicators of the two are relatively close, but both are lower than those of Example 1 containing organosilane impurities and Comparative Example 5 containing methyl silicone oil, indicating that the bridging effect of a small amount of organosilane impurities in the organosilicon slag also has a positive significance for the reinforcement of recycled aggregate.

[0097] (V) Comparison of the performance of recycled aggregates and natural limestone using different treatment processes

[0098] 1. Sample Preparation

[0099] Comparative Example 7

[0100] A construction waste recycled aggregate, namely the recycled aggregate after surface impurities are removed by ultrasonic cleaning as described in step S4 of embodiment 1.

[0101] Comparative Example 8

[0102] A Class I natural limestone crushed stone for construction.

[0103] 2. Performance test:

[0104] The samples obtained in Comparative Examples 7 to 8 were tested for their water absorption and crushing index according to the method described in GB / T 14685-2022 "Pebble and crushed stone for construction".

[0105] The above samples were prepared into C30 concrete specimens, and the basic mix ratio of the C30 concrete specimens was the same as above. Then, the 28d compressive strength of the concrete specimens was tested according to the method described in GB / T 50081-2019 "Standard for Test Methods of Mechanical Properties of Ordinary Concrete".

[0106] The test results are shown in Table 5.

[0107] Table 5 Performance test of Example 1 and Comparative Examples 6 to 7

[0108] Performance Indicators Water absorption / % Crushing index / % Compressive strength / MPa Example 1 0.9 10 39.1 Comparative Example 7 8.3 17 24.5 Comparative Example 8 0.7 6 43.5

[0109] As shown in Table 5, the indicators of Class I natural limestone for construction in Comparative Example 8 are the best, and the maximum compressive strength can reach 43.5MPa. The performance of the recycled aggregate in Comparative Example 7 treated only with ultrasonic cleaning is poor, with a water absorption rate of 8.3%, a crushing index of 17, and a compressive strength of only 24.5MPa. The performance of the recycled aggregate in Example 1 reinforced with organosilicon slag and magnesium slag is significantly improved, approaching the indicators of natural limestone.

[0110] In summary, the organosilicon slag and magnesium slag composite reinforced recycled aggregate provided by the present invention greatly improves the performance indicators of construction waste recycled aggregate, making it close to the indicators of natural limestone gravel, greatly improving the application scope of recycled aggregate, and has good social and environmental benefits.

[0111] The above is a description of a preferred embodiment of the present invention, but it should be understood that the invention is not limited to the contents disclosed herein. As long as non-substantial improvements are made using the method concept and technical solution of the present invention, or the method concept and technical solution of the present invention are applied to other occasions, they are all within the scope of protection of the present invention.

Claims

1. A method for preparing organic silicon slag and magnesium slag composite reinforced recycled aggregate, characterized in that: The following steps are involved: S1: mixing and wet-grinding the organosilicon slag, water and an alcoholamine grinding aid to obtain an organosilicon slag slurry; S2: Dry-grinding the magnesium slag and the alcoholamine grinding aid to obtain magnesium slag powder; S3: Mixing magnesium slag powder, organosilicon slag slurry and water evenly to obtain a suspension; S4: soaking the recycled aggregate in water, ultrasonically cleaning to remove surface impurities, then taking out and soaking in the suspension obtained in step S3, stirring at 100-300r / h for 24-48h, and drying naturally after soaking to obtain a composite reinforced recycled aggregate of organic silicon slag and magnesium slag.

2. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 1, characterized in that: The alcoholamine grinding aid is at least one of triethanolamine, triisopropanolamine and diethanol monoisopropanolamine.

3. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 2, characterized in that: In step S1, the weight ratio of water to organosilicon slag is (0.45-0.60):1, and the amount of alcoholamine grinding aid is 0.5%-1.0% of the mass of the organosilicon slag.

4. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 1, characterized in that: The amount of the alcohol amine grinding aid in step S2 is 0.5% to 2% of the mass of the magnesium slag.

5. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 1, characterized in that: The weight ratio of the magnesium slag powder, the organosilicon slag slurry and the water in step S3 is 1: (3-5): (60-80).

6. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 3, characterized in that: The mass fraction of silicon dioxide in the organic silicon slag in step S1 is not less than 99%.

7. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 6, characterized in that: The wet grinding time in step S1 is 1 to 2 hours, and the wet grinding is performed until the average particle size of the organic silicon slag is 50 to 100 nm.

8. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 4, characterized in that: The dry grinding time in step S2 is 30 to 60 minutes, and the dry grinding is performed until the average particle size of the magnesium slag is 10 to 20 μm.

9. The method for preparing the composite reinforced recycled aggregate of organosilicon slag and magnesium slag according to claim 1, characterized in that: The ultrasonic frequency in step S4 is 20 to 100 kHz, and the time is 10 to 20 minutes.

10. The organic silicon slag and magnesium slag composite reinforced recycled aggregate prepared by the preparation method according to any one of claims 1 to 9.

Citation Information

Patent Citations

  • Method of preparing highly pure silicon dioxide from silicon slag

    CN108516556A

  • Method for preparing heat-insulation mortar through organic silicone waste

    CN109928690A

  • Method for strengthening recycled aggregate and improving bonding of recycled aggregate with mortar

    CN110759657A

  • Recycled aggregate concrete and preparation method thereof

    CN111393094A

  • Preparation method of modified recycled coarse aggregate

    CN112341029A