Lightweight foamed concrete and preparation method thereof
By using modified stearate waterproofing agent in foamed concrete, the shrinkage and cracking problems caused by moisture evaporation are solved, the strength and aesthetics of the material are improved, the strength and beauty of the cement aggregate bonding strength is enhanced, and the water absorption rate is reduced.
Patent Information
- Application Number
- CN202411112213.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-14
- Publication Date
- 2024-11-22
AI Technical Summary
During the curing process, existing foamed concrete shrinks due to moisture evaporation and chemical reaction, which is prone to surface cracking, affecting its aesthetics and reducing its strength and insulation properties.
Use silicate cement, fine sand, water, anionic foaming agent, water reducer, foam stabilizer and polypropylene fiber to combine it into foam concrete, and modify stearate to modified stearate Waterproofing agents enhance the stability and compatibility of the material and reduce water absorption and cracking.
It improves the strength and aesthetics of foamed concrete, reduces water absorption, reduces volume changes and cracks caused by moisture penetration, and enhances the bonding strength between cement material and aggregate.
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of foamed concrete, in particular to lightweight foamed concrete and a preparation method thereof. Background Art
[0002] Foamed concrete, also known as foamed cement, lightweight concrete, etc., is a new type of building energy-saving material that is waste-recycling, environmentally friendly, energy-saving, low-cost and non-flammable. Lightweight concrete (foamed concrete) is a concrete product with a large number of tiny closed pores and considerable strength formed by introducing air or nitrogen, carbon dioxide, oxygen and other gases into the concrete slurry through chemical or physical means according to application needs and then properly cured and formed.
[0003] However, the existing foamed concrete still has the following defects:
[0004] During the curing process of foam concrete, the evaporation of water and chemical reactions will cause the foam concrete to shrink, which will make the surface of the foam concrete prone to cracking. Cracking not only affects the appearance, but also causes the foam concrete material to absorb a large amount of external moisture, further reducing its strength and thermal insulation performance. Summary of the invention
[0005] The object of the present invention is to provide a lightweight foamed concrete and a preparation method thereof, so as to solve the problems raised in the above background technology.
[0006] To achieve the above-mentioned purpose, according to a first aspect of the present invention, a lightweight foamed concrete is provided, which is composed of the following raw materials, in parts by weight: 120-140 parts of silicate cement, 300-340 parts of fine sand, 180-200 parts of water, 220-240 parts of anionic foaming agent, 3-5 parts of water reducer, 25-27 parts of foam stabilizer, 5-10 parts of modified stearate waterproofing agent, and 25-30 parts of polypropylene fiber.
[0007] According to an embodiment of the present invention, the specific preparation method of the modified stearate waterproofing agent is:
[0008] Dissolving stearate in a solvent to form a uniform solution;
[0009] At 70-80°C, slowly add silane coupling agent and catalyst to the solution while stirring. After the silane coupling agent is added, continue stirring for 3 hours. During the stirring process, maintain the pH value between 6-7.
[0010] After the reaction is completed, the mixture is cooled to room temperature, and then the reaction product is washed with deionized water to remove unreacted silane coupling agent;
[0011] Then drying is performed to obtain a modified stearate waterproofing agent.
[0012] According to an embodiment of the present invention, the stearate is one of sodium stearate and magnesium stearate.
[0013] According to an embodiment of the present invention, the silane coupling agent is one of 3-aminopropyltriethoxysilane and 3-glycidyloxypropyltrimethoxysilane.
[0014] According to an embodiment of the present invention, the solvent is one of anhydrous ethanol and isopropanol.
[0015] According to an embodiment of the present invention, the catalyst is one of hydrochloric acid and acetic acid.
[0016] According to an embodiment of the present invention, the anionic foaming agent includes alkyl sulfate and alkyl sulfonate, and the mass ratio of the alkyl sulfate to the alkyl sulfonate is 1:1.
[0017] According to an embodiment of the present invention, the water reducer is one of a naphthalene-based high-efficiency water reducer, a polycarboxylic acid high-efficiency water reducer and a lignin water reducer.
[0018] According to an embodiment of the present invention, the foam stabilizer includes polyacrylamide, polyvinyl alcohol, starch and cellulose, and the mass ratio of the polyacrylamide, polyvinyl alcohol, starch and cellulose is 5:2:1:1.
[0019] According to a second aspect of the present invention, there is provided a method for preparing lightweight foamed concrete, comprising the following steps:
[0020] Step 1, first prepare a modified stearate waterproofing agent;
[0021] Step 2: Weigh silicate cement, fine sand, water, anionic foaming agent, water reducing agent, foam stabilizer, modified stearate waterproofing agent and polypropylene fiber respectively by weight;
[0022] Step 3, uniformly mixing the anionic foaming agent and water, stirring with a foaming machine to generate foam, and obtaining a foam solution;
[0023] Step 4: Mix the Portland cement and fine sand evenly to ensure that there are no lumps, and obtain a dry material mixture;
[0024] Step 5: adding a water reducing agent, a modified stearate waterproofing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, and finally adding a foam stabilizer, stirring evenly, to obtain foamed concrete;
[0025] Step 6: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
[0026] Compared with the prior art, the present invention has the following beneficial effects:
[0027] The present invention combines silicate cement, fine sand, water, anionic foaming agent, water reducing agent, foam stabilizer, modified stearate waterproofing agent and polypropylene fiber into foamed concrete. By modifying stearate into the modified stearate waterproofing agent, the stability and durability of stearate and the compatibility with other components can be increased, thereby enhancing the bonding strength between the cement material and the aggregate, thereby enhancing the strength of the foamed concrete, and reducing the water absorption of the foamed concrete, thereby reducing the volume change and cracks caused by water penetration, avoiding cracking on the surface of the foamed concrete, and ensuring the overall aesthetics of the foamed concrete. DETAILED DESCRIPTION
[0028] The technical solutions in the embodiments of the present invention are described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0029] Example 1
[0030] A method for preparing lightweight foamed concrete comprises the following steps:
[0031] Step 1, first prepare a modified stearate waterproofing agent: dissolve stearate in a solvent to form a uniform solution; slowly add a silane coupling agent and a catalyst to the solution at 70-80°C, stirring while adding, and continue stirring for 3 hours after the silane coupling agent is added. During the stirring process, the pH value is maintained between 6 and 7; after the reaction is completed, cool to room temperature, and then wash the reaction product with deionized water to remove unreacted silane coupling agent; then dry to obtain a modified stearate waterproofing agent;
[0032] Step 2: Weigh 140 parts of Portland cement, 330 parts of fine sand, 200 parts of water, 110 parts of alkyl sulfate, 110 parts of alkyl sulfonate, 4 parts of naphthalene-based high-efficiency water reducer, 15 parts of polyacrylamide, 6 parts of polyvinyl alcohol, 3 parts of starch and 3 parts of cellulose, 5 parts of modified stearate waterproofing agent, and 28 parts of polypropylene fiber respectively by weight;
[0033] Step 3, uniformly mixing the alkyl sulfate, alkyl sulfonate and water, and stirring with a foaming machine to generate foam to obtain a foam solution;
[0034] Step 4: Mix the Portland cement and fine sand evenly to ensure that there are no lumps, and obtain a dry material mixture;
[0035] Step 5, adding naphthalene-based high-efficiency water-reducing agent, modified stearate waterproofing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, finally adding polyacrylamide, polyvinyl alcohol, starch and cellulose, and stirring evenly to obtain foamed concrete;
[0036] Step 6: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
[0037] Example 2
[0038] A method for preparing lightweight foamed concrete comprises the following steps:
[0039] Step 1, first prepare a modified stearate waterproofing agent: dissolve stearate in a solvent to form a uniform solution; slowly add a silane coupling agent and a catalyst to the solution at 70-80°C, stirring while adding, and continue stirring for 3 hours after the silane coupling agent is added. During the stirring process, the pH value is maintained between 6 and 7; after the reaction is completed, cool to room temperature, and then wash the reaction product with deionized water to remove unreacted silane coupling agent; then dry to obtain a modified stearate waterproofing agent;
[0040] Step 2: Weigh 140 parts of Portland cement, 330 parts of fine sand, 200 parts of water, 110 parts of alkyl sulfate, 110 parts of alkyl sulfonate, 4 parts of naphthalene-based high-efficiency water reducer, 15 parts of polyacrylamide, 6 parts of polyvinyl alcohol, 3 parts of starch and 3 parts of cellulose, 10 parts of modified stearate waterproofing agent, and 28 parts of polypropylene fiber respectively by weight;
[0041] Step 3, uniformly mixing the alkyl sulfate, alkyl sulfonate and water, and stirring with a foaming machine to generate foam to obtain a foam solution;
[0042] Step 4: Mix the Portland cement and fine sand evenly to ensure that there are no lumps, and obtain a dry material mixture;
[0043] Step 5, adding naphthalene-based high-efficiency water-reducing agent, modified stearate waterproofing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, finally adding polyacrylamide, polyvinyl alcohol, starch and cellulose, and stirring evenly to obtain foamed concrete;
[0044] Step 6: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
[0045] Comparative Example 1
[0046] A method for preparing lightweight foamed concrete comprises the following steps:
[0047] Step 1: Weigh 140 parts of Portland cement, 330 parts of fine sand, 200 parts of water, 110 parts of alkyl sulfate, 110 parts of alkyl sulfonate, 4 parts of naphthalene-based high-efficiency water reducer, 15 parts of polyacrylamide, 6 parts of polyvinyl alcohol, 3 parts of starch and 3 parts of cellulose, 5 parts of stearate waterproofing agent, and 28 parts of polypropylene fiber respectively by weight;
[0048] Step 2, uniformly mixing the alkyl sulfate, alkyl sulfonate and water, and stirring with a foaming machine to generate foam to obtain a foam solution;
[0049] Step 3, evenly mix the silicate cement and fine sand to ensure that there are no lumps, and obtain a dry material mixture;
[0050] Step 4: adding naphthalene-based high-efficiency water-reducing agent, stearate waterproofing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, and finally adding polyacrylamide, polyvinyl alcohol, starch and cellulose, and stirring evenly to obtain foamed concrete;
[0051] Step 5: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
[0052] The difference between this comparative example and Example 1 is that the modified stearate waterproofing agent is replaced with an unmodified stearate waterproofing agent, and the other components and preparation processes are the same.
[0053] Comparative Example 2
[0054] A method for preparing lightweight foamed concrete comprises the following steps:
[0055] Step 1: Weigh 140 parts of Portland cement, 330 parts of fine sand, 200 parts of water, 110 parts of alkyl sulfate, 110 parts of alkyl sulfonate, 4 parts of naphthalene-based high-efficiency water reducer, 15 parts of polyacrylamide, 6 parts of polyvinyl alcohol, 3 parts of starch, 3 parts of cellulose, and 28 parts of polypropylene fiber respectively by weight;
[0056] Step 2, uniformly mixing the alkyl sulfate, alkyl sulfonate and water, and stirring with a foaming machine to generate foam to obtain a foam solution;
[0057] Step 3, evenly mix the silicate cement and fine sand to ensure that there are no lumps, and obtain a dry material mixture;
[0058] Step 4: adding naphthalene-based high-efficiency water reducing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, and finally adding polyacrylamide, polyvinyl alcohol, starch and cellulose, and stirring evenly to obtain foamed concrete;
[0059] Step 5: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
[0060] The difference between this comparative example and Example 1 is that the modified stearate waterproofing agent is omitted, and the other components and preparation processes are the same.
[0061] Experimental example
[0062] The lightweight foamed concrete prepared in Example 1-2 and the foamed concrete prepared in Comparative Example 1-2 were subjected to performance tests, and the test results are shown in Table 1:
[0063] Table 1 Performance test
[0064] Compressive strength(MPa) Water absorption (%) Technical requirements Comply with the provisions of JG / T266-2011 Comply with the provisions of JG / T266-2011 Example 1 5.6 6 Example 2 7.4 4 Comparative Example 1 4.8 10 Comparative Example 2 2.7 14
[0065] As can be seen from the above table, the performance indicators of the foamed concrete prepared in Examples 1-2 of the present application meet the requirements of JG / T266-2011, and are better than the data of the foamed concrete prepared in Comparative Examples 1-2;
[0066] By comparing the data of Example 1 and Comparative Example 1, it can be seen that when the modified stearate waterproofing agent is replaced with the unmodified stearate waterproofing agent, the compressive strength of the foamed concrete decreases and the water absorption rate increases. Therefore, by replacing the unmodified stearate waterproofing agent with the modified stearate waterproofing agent, the stability, durability and compatibility of the stearate with other components can be increased, thereby enhancing the bonding strength between the cement material and the aggregate, thereby enhancing the strength of the foamed concrete, and reducing the water absorption of the foamed concrete, thereby reducing the volume change and cracks caused by water penetration;
[0067] By comparing the data of Example 1 and Comparative Example 2, it can be seen that in the absence of the modified stearate waterproofing agent, the compressive strength of the foamed concrete is significantly reduced and the water absorption rate is significantly increased. Therefore, by adding the modified stearate waterproofing agent, the compressive strength of the foamed concrete can be significantly improved, and the water absorption rate of the foamed concrete can be significantly reduced;
[0068] In summary, the present invention combines silicate cement, fine sand, water, anionic foaming agent, water reducer, foam stabilizer, modified stearate waterproofing agent and polypropylene fiber into foamed concrete. By modifying stearate into modified stearate waterproofing agent, the stability, durability and compatibility of stearate with other components can be increased, thereby enhancing the bonding strength between cement material and aggregate, thereby enhancing the strength of foamed concrete, and reducing the water absorption of foamed concrete, thereby reducing volume changes and cracks caused by water penetration, avoiding cracking on the surface of foamed concrete, and ensuring the overall aesthetics of foamed concrete.
[0069] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A lightweight foamed concrete, It is characterized in that The invention is composed of the following raw materials in parts by weight: 120-140 parts of silicate cement, 300-340 parts of fine sand, 180-200 parts of water, 220-240 parts of anionic foaming agent, 3-5 parts of water reducer, 25-27 parts of foam stabilizer, 5-10 parts of modified stearate waterproofing agent and 25-30 parts of polypropylene fiber.
2. A lightweight foamed concrete according to claim 1, It is characterized in that The specific preparation method of the modified stearate waterproofing agent is: Dissolving stearate in a solvent to form a uniform solution; At 70-80°C, slowly add silane coupling agent and catalyst to the solution while stirring. After the silane coupling agent is added, continue stirring for 3 hours. During the stirring process, maintain the pH value between 6-7. After the reaction is completed, the mixture is cooled to room temperature, and then the reaction product is washed with deionized water to remove unreacted silane coupling agent; Then drying is performed to obtain a modified stearate waterproofing agent.
3. A lightweight foamed concrete according to claim 2, It is characterized in that The stearate is one of sodium stearate and magnesium stearate.
4. A lightweight foamed concrete according to claim 2, It is characterized in that The silane coupling agent is one of 3-aminopropyltriethoxysilane and 3-glycidyloxypropyltrimethoxysilane.
5. A lightweight foamed concrete according to claim 2, It is characterized in that The solvent is one of anhydrous ethanol and isopropanol.
6. A lightweight foamed concrete according to claim 2, It is characterized in that The catalyst is one of hydrochloric acid and acetic acid.
7. The lightweight foamed concrete according to claim 1, It is characterized in that The anionic foaming agent includes alkyl sulfate and alkyl sulfonate, and the mass ratio of the alkyl sulfate to the alkyl sulfonate is 1:
1.
8. The lightweight foamed concrete according to claim 1, It is characterized in that The water reducer is one of a naphthalene-based high-efficiency water reducer, a polycarboxylic acid high-efficiency water reducer and a lignin water reducer.
9. The lightweight foamed concrete according to claim 1, It is characterized in that The foam stabilizer comprises polyacrylamide, polyvinyl alcohol, starch and cellulose, and the mass ratio of the polyacrylamide, polyvinyl alcohol, starch and cellulose is 5:2:1:
1.
10. A method for preparing lightweight foamed concrete according to any one of claims 1 to 9, It is characterized in that The following steps are involved: Step 1, first prepare a modified stearate waterproofing agent; Step 2: Weigh silicate cement, fine sand, water, anionic foaming agent, water reducing agent, foam stabilizer, modified stearate waterproofing agent and polypropylene fiber respectively by weight; Step 3, uniformly mixing the anionic foaming agent and water, stirring with a foaming machine to generate foam, and obtaining a foam solution; Step 4: Mix the Portland cement and fine sand evenly to ensure that there are no lumps, and obtain a dry material mixture; Step 5: adding a water reducing agent, a modified stearate waterproofing agent and polypropylene fiber to the dry material mixture, stirring evenly, then slowly adding the foam solution to the dry material mixture, stirring until the foam is evenly distributed, and finally adding a foam stabilizer, stirring evenly, to obtain foamed concrete; Step 6: Pour the above foamed concrete into a mold, compact it by vibration, and cure it at room temperature for 24 hours. After the foamed concrete solidifies and is demolded, lightweight foamed concrete is obtained.
Citation Information
Cited By
Waterproof, anti-crack and moisture-proof self-healing material for concrete structure and preparation method of self-healing material
CN119750963A