High-strength tundish dry material and preparation method thereof
Through the synergistic effect of components such as sintered magnesium sand, modified hydroxyapatite, silica fume and phenolic resin, the problem of insufficient strength of the sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered sintered Stable operation and extended service life.
Patent Information
- Application Number
- CN202411177372.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-08-26
AI Technical Summary
Traditional lumpy materials are difficult to operate stably in harsh environments due to insufficient strength during the efficient continuous casting process, and are prone to cracks and peeling, which cannot meet the harsh working conditions requirements.
Using sintered magnesium sand, modified hydroxyapatite, silica fume, phenolic resin and polymeric iron sulfate, the synergistic action of organic polymer and inorganic polymer, a high-strength crumb-type material is formed to improve its room temperature resistance. Pressure strength.
It significantly improves the room temperature and compressive strength of the slag-type material, ensures stable operation in harsh environments, extends service life, and is simple to prepare and suitable environment.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of refractory materials, and in particular to a high-strength tundish dry material and a preparation method thereof. Background Art
[0002] In the steel production process, the tundish plays a vital role as a transition device from the ladle to the crystallizer. As the lining material of the tundish, the performance of the tundish dry material is directly related to the overall performance and service life of the tundish. For example, if the strength of the tundish dry material is insufficient, it is easy to crack and peel under frequent thermal shock and mechanical vibration.
[0003] With the continuous promotion of efficient continuous casting technology, the working conditions of the tundish have become more demanding. The strength of the traditional tundish dry material can no longer meet the market demand. It is urgent to develop a tundish dry material with higher strength to ensure that the tundish can operate stably in harsh environments. Summary of the invention
[0004] The invention provides a high-strength tundish dry material and a preparation method thereof, which solves the problem of poor room-temperature compressive strength of the tundish dry material in the related art.
[0005] The technical solution of the present invention is as follows: The present invention provides a high-strength tundish dry material, comprising the following components in parts by weight: 150 parts of sintered magnesia, 40-60 parts of hydroxyapatite, 20-40 parts of silica fume, 8-12 parts of a binder, and 0.5-1 part of a curing agent; The binder includes phenolic resin and polyferric sulfate.
[0006] As a further technical solution, the weight ratio of the phenolic resin to the polyferric sulfate is 3:2~9:1.
[0007] In the present invention, when the weight ratio of the phenolic resin to the polyferric sulfate is 3:2-9:1, it helps to further improve the room temperature compressive strength of the tundish dry material.
[0008] As a further technical solution, the hydroxyapatite is modified hydroxyapatite.
[0009] In the present invention, by modifying hydroxyapatite, the bonding between hydroxyapatite and sintered magnesia during sintering can be enhanced, and the densification of the tundish dry material can be further promoted, thereby further improving the room temperature compressive strength of the tundish dry material.
[0010] As a further technical solution, the modified hydroxyapatite comprises the following components: hydroxyapatite, ferrous acetylacetonate and ferrous stearate.
[0011] In the present invention, the inventors found that the room temperature compressive strength of the tundish dry material can be further improved by modifying hydroxyapatite with ferrous acetylacetonate and ferrous stearate. It is speculated that this is because ferrous acetylacetonate and ferrous stearate can improve the sintering activity of hydroxyapatite and promote the combination of hydroxyapatite and sintered magnesia.
[0012] As a further technical solution, the preparation method of the modified hydroxyapatite comprises the following steps: dissolving ferric acetylacetonate and ferric stearate in ethanol, adding hydroxyapatite, dispersing evenly, and drying to obtain the modified hydroxyapatite.
[0013] As a further technical solution, the weight ratio of the hydroxyapatite to ferrous acetylacetonate and ferrous stearate is 10.5-13:1:1.
[0014] In the present invention, when the weight ratio of hydroxyapatite to ferrous acetylacetonate and ferrous stearate is 10.5-13:1:1, it helps to further improve the room temperature compressive strength of the tundish dry material.
[0015] As a further technical solution, the temperature during the dissolution is 40-50°C.
[0016] As a further technical solution, the particle sizes of the sintered magnesia, hydroxyapatite and silica fume are independently 100-600 meshes.
[0017] As a further technical solution, the particle size of the sintered magnesia is 100-200 mesh; and / or The particle size of the hydroxyapatite is 250-325 mesh; and / or The particle size of the silica fume is 400-600 mesh.
[0018] In the present invention, by designing the particle size distribution of sintered magnesia, hydroxyapatite and silica fume, the compactness of the tundish dry material can be improved, and the room temperature compressive strength of the tundish dry material can be further improved.
[0019] As a further technical solution, the mass fraction of magnesium oxide in the sintered magnesia is ≥95%.
[0020] As a further technical solution, the mass fraction of silicon dioxide in the silica ash is ≥95%.
[0021] As a further technical solution, the curing agent includes one of hexamethylenetetramine, p-toluenesulfonic acid, and 2-methylimidazole.
[0022] The present invention also provides a method for preparing the high-strength tundish dry material, which comprises the following steps: mixing the components uniformly to obtain the tundish dry material.
[0023] The working principle and beneficial effects of the present invention are: In the present invention, the tundish dry material has the advantages of easy raw material availability, simple preparation and good construction environment, etc. Among them, phenolic resin and polyferric sulfate are used as binders, and through the synergistic effect of organic polymers and inorganic polymers, the tundish dry material can form a firm three-dimensional grid structure after baking, which significantly improves the room temperature compressive strength of the tundish dry material. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0025] In the following embodiments and comparative examples, unless otherwise specified, the particle size of sintered magnesia is 100 mesh, and the mass fraction of magnesium oxide is 95.16%; the particle size of hydroxyapatite is 325 mesh, and the calcium-phosphorus ratio is 1.67; the particle size of silica fume is 600 mesh, and the content of silicon dioxide is 98.24%; the model of phenolic resin is PF-2123; and the model of polyferric sulfate is YT-0104.
[0026] Example 1 A method for preparing a high-strength tundish dry material comprises the following steps: by weight, 150 parts of sintered magnesia, 40 parts of hydroxyapatite, 20 parts of silica fume, 4 parts of phenolic resin, 4 parts of polymerized ferric sulfate and 0.5 parts of hexamethylenetetramine are mixed evenly to obtain a tundish dry material.
[0027] Example 2 A method for preparing a high-strength tundish dry material comprises the following steps: by weight, 150 parts of sintered magnesia, 60 parts of hydroxyapatite, 40 parts of silica fume, 6 parts of phenolic resin, 6 parts of polymerized ferric sulfate and 1 part of hexamethylenetetramine are uniformly mixed to obtain a tundish dry material.
[0028] Example 3 A method for preparing a high-strength tundish dry material comprises the following steps: by weight, 150 parts of sintered magnesia, 50 parts of hydroxyapatite, 30 parts of silica fume, 5 parts of phenolic resin, 5 parts of polymerized ferric sulfate and 0.75 parts of hexamethylenetetramine are mixed uniformly to obtain a tundish dry material.
[0029] Example 4 The only difference between this embodiment and embodiment 3 is that, in this embodiment, the weight portion of phenolic resin is 9.5 parts, and the weight portion of polyferric sulfate is 0.5 parts.
[0030] Example 5 The only difference between this embodiment and embodiment 3 is that in this embodiment, the weight parts of phenolic resin are 6 parts and the weight parts of polyferric sulfate are 4 parts.
[0031] Example 6 The only difference between this embodiment and embodiment 3 is that in this embodiment, the weight portion of phenolic resin is 9 parts, and the weight portion of polyferric sulfate is 1 part.
[0032] Example 7 The only difference between this embodiment and embodiment 6 is that in this embodiment, the hydroxyapatite is modified hydroxyapatite, and the preparation method of the modified hydroxyapatite includes the following steps: dissolving 2 parts of iron stearate in ethanol at 45°C, adding 48 parts of hydroxyapatite, dispersing evenly, and drying to obtain modified hydroxyapatite.
[0033] Example 8 The only difference between this embodiment and embodiment 6 is that in this embodiment, the hydroxyapatite is modified hydroxyapatite, and the preparation method of the modified hydroxyapatite includes the following steps: dissolving 2 parts of ferric acetylacetonate in ethanol at 45°C, adding 48 parts of hydroxyapatite, dispersing evenly, and drying to obtain modified hydroxyapatite.
[0034] Example 9 The only difference between this embodiment and embodiment 6 is that in this embodiment, the hydroxyapatite is modified hydroxyapatite, and the preparation method of the modified hydroxyapatite includes the following steps: dissolving 1 part of ferric acetylacetonate and 1 part of ferric stearate in ethanol at 45°C, adding 48 parts of hydroxyapatite, dispersing evenly, and drying to obtain modified hydroxyapatite.
[0035] Example 10 The only difference between this embodiment and embodiment 9 is that in this embodiment, when preparing modified hydroxyapatite, the weight parts of ferric acetylacetonate are 5 parts, the weight parts of iron stearate are 5 parts, and the weight parts of hydroxyapatite are 40 parts.
[0036] Embodiment 11 The only difference between Example 1 and Example 9 is that in this example, when preparing modified hydroxyapatite, the weight parts of ferric acetylacetonate are 2 parts, the weight parts of iron stearate are 2 parts, and the weight parts of hydroxyapatite are 46 parts.
[0037] Example 12 The only difference between Example 1 and Example 9 is that in this example, when preparing modified hydroxyapatite, the weight parts of ferric acetylacetonate are 4 parts, the weight parts of iron stearate are 4 parts, and the weight parts of hydroxyapatite are 42 parts.
[0038] Comparative Example 1 The difference between this comparative example and Example 1 is that in this comparative example, no polyferric sulfate is added and the weight portion of the added phenolic resin is 8 parts.
[0039] Comparative Example 2 The difference between this comparative example and Example 1 is that in this comparative example, no phenolic resin is added and the weight portion of the added polyferric sulfate is 8 parts.
[0040] Comparative Example 3 The difference between this comparative example and Example 1 is that, in this comparative example, the polyferric sulfate is replaced by an equal amount of ferric sulfate.
[0041] The tundish dry vibrating materials prepared in Examples 1 to 12 and Comparative Examples 1 to 3 were prepared into samples according to the provisions of GB / T 4513.5-2017 "Monomorphous Refractory Materials Part 5: Sample Preparation and Pretreatment", with the sample size of 50 mm in diameter and 50 mm in height, and then the following performance tests were carried out: ① Room temperature compressive strength after sintering at 200℃ for 2h: room temperature compressive strength is measured in accordance with GB / T 4513.6-2017 "Monomorphous Refractory Materials Part 6: Determination of Physical Properties"; ② Room temperature compressive strength after sintering at 1500℃ for 3h: The room temperature compressive strength is determined in accordance with GB / T 4513.6-2017 "Monomorphous Refractory Materials Part 6: Determination of Physical Properties".
[0042] The test results are shown in Table 1 below.
[0043] Table 1 Test results of room temperature compressive strength
[0044] The comparison between Example 1 and Comparative Examples 1 to 3 shows that the room temperature compressive strength of the tundish dry material can be significantly improved by the synergistic effect of the phenolic resin and polyferric sulfate as binders. The comparison between Examples 3 to 4 and Examples 5 to 6 shows that when the weight ratio of phenolic resin to polyferric sulfate is 3:2 to 9:1, it helps to further improve the room temperature compressive strength of the tundish dry material. The comparison between Example 6 and Examples 7 to 12 shows that by modifying hydroxyapatite, the room temperature compressive strength of the tundish dry material is further improved. The comparison between Examples 7 to 8 and Example 9 shows that by modifying hydroxyapatite with ferrous acetylacetonate and ferrous stearate, the room temperature compressive strength of the tundish dry material can be further improved. The comparison between Examples 9 to 10 and Examples 11 to 12 shows that when the weight ratio of hydroxyapatite to ferrous acetylacetonate and ferrous stearate is 10.5 to 13:1:1, it helps to further improve the room temperature compressive strength of the tundish dry material.
[0045] The above are only preferred embodiments of the present invention and are not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.
Claims
1. A high-strength tundish dry material, characterized in that: The invention comprises the following components in parts by weight: 150 parts of sintered magnesia, 40-60 parts of hydroxyapatite, 20-40 parts of silica fume, 8-12 parts of a binder, and 0.5-1 part of a curing agent; The binder includes phenolic resin and polyferric sulfate.
2. The high-strength tundish dry material according to claim 1, characterized in that: The weight ratio of the phenolic resin to the polyferric sulfate is 3:2-9:
1.
3. The high-strength tundish dry material according to claim 1, characterized in that: The hydroxyapatite is modified hydroxyapatite.
4. The high-strength tundish dry material according to claim 3, characterized in that: The modified hydroxyapatite comprises the following components: hydroxyapatite, iron acetylacetonate and iron stearate.
5. The high-strength tundish dry material according to claim 4, characterized in that: The preparation method of the modified hydroxyapatite comprises the following steps: dissolving ferric acetylacetonate and ferric stearate in ethanol, adding hydroxyapatite, dispersing evenly, and drying to obtain the modified hydroxyapatite.
6. The high-strength tundish dry material according to claim 4, characterized in that: The weight ratio of the hydroxyapatite to ferrous acetylacetonate and ferrous stearate is 10.5-13:1:
1.
7. The high-strength tundish dry material according to claim 1, characterized in that: The particle sizes of the sintered magnesia, hydroxyapatite and silica fume are independently 100-600 meshes.
8. The high-strength tundish dry material according to claim 7, characterized in that: The particle size of the sintered magnesia is 100-200 mesh; and / or The particle size of the hydroxyapatite is 250-325 mesh; and / or The particle size of the silica fume is 400-600 mesh.
9. The high-strength tundish dry material according to claim 1, characterized in that: The curing agent includes one of hexamethylenetetramine, p-toluenesulfonic acid and 2-methylimidazole.
10. A method for preparing a high-strength tundish dry material according to any one of claims 1 to 9, characterized in that: The following steps are involved: The components are mixed evenly to obtain a tundish dry material.
Citation Information
Patent Citations
Sludge solidifier and preparation method thereof
CN108314280A
Composite material with air purification function and preparation method thereof
CN113262632A
Tundish dry material added with zircon powder and preparation method thereof
CN114292089A
Ceramic tile with leaf surface and preparation method thereof
CN114890816A
Water purifying agent for sewage treatment as well as preparation method and application of water purifying agent