Preparation process of ceramic substrate capable of reducing generation of pinholes and ceramic substrate
By controlling the purity and particle size of alumina powder, using organic solvents and sintering aids, controlling the sintering rate and performing degreasing treatment, the problems of pinholes and ash points of ceramic substrates during sintering are solved, and the quality and stability of the substrate are improved sex.
Patent Information
- Application Number
- CN202411033558.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-30
- Publication Date
- 2024-11-22
AI Technical Summary
Ceramic substrates are prone to pinholes during sintering, which affects their quality, and the prior art is difficult to effectively solve this problem.
By controlling the purity and particle size of the alumina powder, mixing with organic solvents and dispersants, adding sintering aids to form liquid-filled air pores, controlling the sintering temperature increase and cooling rate, reducing the content of flammable and volatile impurities, and reducing the content of flammable and volatile impurities. Gas generation and bubble closure are used to degreasing and separating powder to reduce ash and pockmarks.
The pinholes and gray spots in the ceramic substrate are significantly reduced, the compactness and structural stability of the substrate are improved, and the quality and performance are improved.
Smart Images

Figure CN118993709A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of ceramic substrate preparation technology, and in particular to a ceramic substrate preparation technology and a ceramic substrate capable of reducing the generation of pinholes. Background Art
[0002] In recent years, with the vigorous development of the microelectronics packaging industry, electronic packaging technology has developed in the direction of miniaturization, high density, multi-power and high reliability. Electronic packaging materials have gradually become an industrial field with high technology content, high economic benefits and important status. At present, the commonly used substrate materials are mainly plastic substrates, metal substrates, ceramic substrates and composite substrates. The ultra-thin composite substrate made of advanced ceramic materials has excellent electrical insulation properties, high thermal conductivity, excellent soft soldering and high adhesion strength, and can be etched with various graphics like PCB boards, with great current carrying capacity. Ceramic substrates are widely used in high-power power semiconductor modules, power control circuits, automotive electronics, aerospace and military electronic components, solar panel components and other fields because of their much better heat dissipation performance, current carrying capacity, insulation, thermal expansion coefficient, etc. than ordinary glass fiber PCB boards. At present, the main market share of ceramic substrates with a purity greater than 99% is still occupied by overseas giants such as Kyocera of Japan. Domestic ceramic substrate manufacturers have increased their investment and improved their R&D capabilities, but their R&D capabilities for high-end products still need to be improved. For example, in related technologies, pinholes are prone to appear in finished ceramic substrates, which affects the quality of the ceramic substrates. Summary of the invention
[0003] The main purpose of the present invention is to provide a preparation process of a ceramic substrate and a ceramic substrate for reducing the generation of pinholes, so as to solve the technical problem that pinholes are easily generated in the ceramic substrate.
[0004] To achieve the above object, the present invention provides a process for preparing a ceramic substrate for reducing the generation of pinholes, comprising the following steps:
[0005] S10, preparing slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry, wherein the purity of the alumina powder is ≥99.9%;
[0006] S20, green blank forming: pressing and forming the slurry into a ceramic green blank;
[0007] S30, sintering: placing the ceramic green blank on the surface of a sintering plate, heating the ceramic green blank at a heating rate of 0.1°C / min to 0.5°C / min to perform a sintering treatment, and then cooling the ceramic green blank at a cooling rate of 0.1°C / min to 0.5°C / min to obtain a ceramic substrate.
[0008] In some embodiments of the present invention, the moisture content of the alumina powder is ≤0.1%.
[0009] In some embodiments of the present invention, the purity of the aluminum oxide powder is 99.6% to 99.999%.
[0010] In some embodiments of the present invention, the particle size D50 of the aluminum oxide powder is 0.5 μm to 1.0 μm.
[0011] In some embodiments of the present invention, the organic solvent includes an ester compound and an alcohol compound, wherein the ester compound includes at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate; and / or the alcohol compound includes at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.
[0012] In some embodiments of the present invention, the organic solvent includes an alcohol compound and an ester compound, and the mass ratio of the alcohol compound to the ester compound is (7-9):(1-3).
[0013] In some embodiments of the present invention, the dispersant comprises triolein;
[0014] and / or, the plasticizer comprises at least one of dibutyl phthalate and polyethylene glycol;
[0015] And / or, the binder comprises polyvinyl butyral.
[0016] In some embodiments of the present invention, the setter plate comprises an alumina setter plate; and / or the purity of the setter plate is ≥99.9%.
[0017] In some embodiments of the present invention, in the sintering step, the temperature is lowered to 800° C. to 1000° C. at a cooling rate of 0.1° C. / min to 0.5° C. / min.
[0018] The present invention also provides a ceramic substrate prepared by the above-mentioned process for preparing the ceramic substrate with reduced pinhole generation.
[0019] The beneficial effects that can be achieved by the present invention are:
[0020] The present invention controls the purity of the raw materials of the ceramic substrate, reduces the content of combustible impurities and volatile impurities in the raw materials, and reduces the occurrence of pinholes in the ceramic substrate caused by excessive generation of gas due to combustible gas and volatile impurities during the sintering process. In addition, the sintering heating rate is controlled during the sintering process to promote gas overflow, and the cooling rate is controlled to cause the closed bubbles to collapse in time, thereby reducing the generation of pinholes in the finished ceramic substrate. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the embodiments or the description of the prior art. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on the structures shown in these drawings without paying creative work.
[0022] Figure 1 The figure is a schematic flow chart of a method for preparing a ceramic substrate of the present invention.
[0023] The realization of the purpose, functional features and advantages of the present invention will be further explained in conjunction with embodiments and with reference to the accompanying drawings. DETAILED DESCRIPTION
[0024] It should be understood that the specific embodiments described herein are only used to explain the present invention, and are not used to limit the present invention.
[0025] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] In the present invention, descriptions such as "first", "second", etc. are only used for descriptive purposes and cannot be understood as indicating or implying their relative importance or implicitly indicating the number of the indicated technical features. Therefore, the features defined as "first" and "second" may explicitly or implicitly include at least one of the features. In addition, the technical solutions between the various embodiments can be combined with each other, but they must be based on the ability of ordinary technicians in the field to implement them. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention.
[0027] In the process of preparing ceramic substrates, the raw material alumina powder has a high purity, and it is difficult to produce a liquid phase during the sintering process, which easily leads to the formation of closed pores. It is also difficult to remove organic matter, thus forming closed pores during the sintering process, which causes gray spots to appear on the ceramic substrate.
[0028] In view of this, the present invention provides a preparation process of a ceramic substrate with reduced pinhole generation, referring to Figure 1 The preparation process comprises the following steps:
[0029] S10, preparing slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry, wherein the purity of the alumina powder is ≥99.9%;
[0030] S20, green blank forming: pressing and forming the slurry into a ceramic green blank;
[0031] S30, sintering: placing the ceramic green blank on the surface of a sintering plate, heating the ceramic green blank at a heating rate of 0.1°C / min to 0.5°C / min to perform a sintering treatment, and then cooling the ceramic green blank at a cooling rate of 0.1°C / min to 0.5°C / min to obtain a ceramic substrate.
[0032] In the present invention, the purity of the alumina powder is ≥99.9%. The higher the purity of the alumina powder, the lower the content of combustible impurities and volatile impurities, and the lower the pinholes in the ceramic substrate caused by excessive generation of combustible gas and volatile impurities during the sintering process.
[0033] In some embodiments, the moisture content of the alumina powder is ≤0.1%, so that during the casting process of the green billet forming stage, pores are not easily formed inside the ceramic substrate due to excessive water vapor that is difficult to be discharged in time.
[0034] In some embodiments, the particle size D50 of the alumina powder is 0.5 μm to 1.0 μm, and can be any value in the range of 0.5 μm to 1.0 μm, such as 0.5 μm, 0.6 μm, 0.7 μm, 0.8 μm, 0.9 μm, 1.0 μm, etc. The alumina powder under the above particle size range conditions is conducive to promoting the dispersion of the alumina powder and sintering to obtain a dense, structurally stable, electromechanically stable, smooth surface, and less gray spots and pitting ceramic substrate.
[0035] In the present invention, the organic solvent plays the role of dissolving the alumina powder and mixing various raw materials.
[0036] In some embodiments, the organic solvent includes an ester compound and an alcohol compound, wherein the ester compound includes at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate; and / or the alcohol compound includes at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol.
[0037] In some embodiments, the mass ratio of alcohol compounds to ester compounds in the organic solvent is (7-9):(1-3), which can be 7:1, 7:2, 7:3, 8:1, 8:2, 8:3, 9:1, 9:2, 9:3.
[0038] In some embodiments, the dispersant includes triolein. Using triolein as a dispersant is beneficial to promoting uniform dispersion of the aluminum oxide powder.
[0039] In the present invention, the plasticizer plays a role in enhancing the strength and toughness of the green porcelain tape.
[0040] In some embodiments, the plasticizer includes at least one of dibutyl phthalate and polyethylene glycol.
[0041] In the present invention, the binder can strengthen the bonding force between various raw materials, which is beneficial to obtain a ceramic substrate with a stable structure, and can also improve the hardness and strength of the ceramic substrate.
[0042] In some embodiments, the binder includes polyvinyl butyral.
[0043] In some embodiments, the purity of the aluminum oxide powder is 99.6% to 99.999%, which can be 99.6%, 99.9%, 99.99%, 99.999%, etc. The purity of aluminum oxide is relatively high, and the content of combustible impurities and volatile impurities therein is relatively low, which can reduce the occurrence of pinholes in the ceramic substrate caused by excessive generation of gas due to combustible gas and volatile impurities during the sintering process. In this embodiment, although increasing the purity of aluminum oxide powder can reduce the occurrence of pinholes, the purity of aluminum oxide powder reaches 99.9% or above, and the high purity will face the problem of difficulty in forming liquid during the sintering process, resulting in the formation of closed pores, thereby causing the formation of gray spots on the finished ceramic substrate.
[0044] Therefore, in some embodiments, in the step of preparing the slurry, in the step of mixing the alumina powder and the dispersant in the organic solvent, a sintering aid can also be added for mixing. The sintering aid can form a liquid phase during the sintering process and has fluidity, and can effectively fill the pores, gaps or defects generated during the sintering process, thereby reducing the generation of closed pores during the sintering process and alleviating the problem of gray spots in the finished ceramic substrate. In this embodiment, alumina powder with a high purity of 99.6% to 99.999% can be used as a raw material to obtain a ceramic substrate with a stable structure, fewer closed pores, and fewer pinholes and gray spots.
[0045] In some embodiments, the sintering aid includes magnesium oxide, which can become a fluid liquid during high-temperature sintering, effectively filling the pores, voids or defects generated during the sintering process, reducing the generation of closed pores in the ceramic substrate, thereby reducing gray spots.
[0046] In some embodiments, the particle size range of the sintering aid is 0.5μm to 1.0μm, and can be any value in the range of 0.5μm to 1.0μm, such as 0.5μm, 0.6μm, 0.7μm, 0.8μm, 0.9μm, 1.0μm, etc. The sintering aid is conducive to matching with the alumina powder under the above particle size range conditions, and is easy to form a liquid with fluidity during high-temperature sintering, and effectively fills the pores, voids or defects generated during the sintering process, which is conducive to sintering to obtain a ceramic substrate with uniform structure, while reducing the generation of closed pores to reduce gray spots in the finished ceramic substrate.
[0047] In some embodiments, the slurry includes the following components, calculated by weight percentage: alumina powder: 40% to 60%; organic solvent: 30% to 45%; dispersant: 1% to 3%; plasticizer: 5% to 10%; binder: 7% to 10%; for example, the alumina powder can be any value in the range of 40% to 60%, such as 40%, 42%, 45%, 48%, 50%, 52%, 55%, 58%, 60%, etc., and the organic solvent can be any value in the range of 40% to 60%. The agent can be any value in the range of 30% to 45%, such as 30%, 35%, 40%, 45%; the dispersant can be any value in the range of 1% to 3%, such as 1%, 2%, 3%; the plasticizer can be any value in the range of 5% to 10%, such as 5%, 6%, 7%, 8%, 9%, 10%; the binder can be any value in the range of 0.35% to 10%, such as 0.35%, 0.5%, 7%, 8%, 9%, 10%.
[0048] In some embodiments, the slurry may further include 0.2% to 1.2% of a sintering aid, calculated as a percentage by weight, which may be any value within the range of 0.2% to 1.2%, such as 0.2%, 0.5%, 0.8%, 1.0%, 1.2%, or the like.
[0049] In the step of preparing the slurry, the alumina powder and the dispersant are first dispersed in the organic solvent, which can enhance the dispersion effect of the alumina powder in the entire slurry system, thereby preparing a ceramic substrate with a stable structure. In some embodiments, a sintering aid can also be added to the alumina powder and the dispersant, and the sintering aid and the alumina powder are evenly dispersed with the help of the dispersant, so that the sintering aid can fully fill the pores, voids or defects generated during the sintering process, thereby reducing the gray spots in the ceramic substrate.
[0050] In some embodiments, after the alumina powder and the dispersant are dispersed in the organic solvent, they can be ball milled and mixed for 20 to 30 hours, for example, 20 hours, 24 hours, 28 hours, 30 hours, etc., to promote uniform dispersion of the alumina powder. In this embodiment, a sintering aid can also be added for ball milling and mixing.
[0051] In some embodiments, after adding the thickener and the binder, the mixture may be further ball-milled to obtain a slurry.
[0052] In some embodiments, the green blank forming process includes the following steps:
[0053] Casting: Casting the slurry into a green porcelain tape;
[0054] Laminated isostatic pressing: The raw porcelain strip is laminated and isostatically pressed to obtain a ceramic blank.
[0055] In the casting step, the thickness of the green porcelain tape can be controlled according to actual needs. In some embodiments, the thickness of the green porcelain tape ranges from 1 μm to 100 μm, and can be 1 μm, 10 μm, 20 μm, 30 μm, 35 μm, 40 μm, 45 μm, 50 μm, 55 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm or other values in the range of 1 μm to 100 μm.
[0056] The laminated isostatic pressing treatment is beneficial for obtaining a high-density and uniform ceramic green body, which reduces the shrinkage of the ceramic green body during the subsequent sintering process and is not prone to deformation.
[0057] In some steps of laminated isostatic pressing, the temperature range of isostatic pressing treatment is 50℃~80℃, and can be any value within the range of 50℃~80℃, such as 50℃, 60℃, 70℃, 80℃, etc. Within the above temperature range of isostatic pressing treatment, it is beneficial to obtain a ceramic green body with high density and uniformity, and the ceramic green body is not prone to shrinkage and deformation.
[0058] In some steps of laminated isostatic pressing, the pressure range of isostatic pressing treatment is 50MPa~100MPa, and can be any value in the range of 50MPa~100MPa, such as 50MPa, 60MPa, 70MPa, 80MPa, 90MPa, 100MPa, etc. Under the above isostatic pressing treatment pressure conditions, a high-density ceramic green body can be obtained, and it is not easy to cause deformation of the ceramic green body.
[0059] In some steps of laminated isostatic pressing, the holding time of the isostatic pressing treatment is 5 minutes to 20 minutes, and can be any value in the range of 5 minutes to 20 minutes, such as 5 minutes, 8 minutes, 10 minutes, 12 minutes, 15 minutes, 18 minutes, 20 minutes, etc. Under the above holding time range conditions, a high-density ceramic green body can be obtained, and it is not easy to cause deformation of the ceramic green body.
[0060] In some embodiments, the ceramic blanks may be stacked before sintering to improve production efficiency. However, direct contact between the ceramic blanks may cause adverse effects such as adhesion during the subsequent sintering process. Therefore, in this embodiment, a layer of isolating powder is provided between any two layers of ceramic blanks. The addition of isolating powder may cause new problems. For example, the isolating powder may react with the ceramic blanks during the sintering process, resulting in pitting on the surface of the ceramic substrate. In this embodiment, the ceramic blanks include degreased ceramic blanks.
[0061] Therefore, in one embodiment, the process steps of powder coating and lamination are as follows: placing more than two layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size range of the insulating powder is 1μm to 100μm. This embodiment selects insulating powder with a purity of ≥99.99% and a particle size range of 1μm to 100μm, which improves the purity of the insulating powder and reduces the risk of pitting on the finished ceramic substrate due to excessive impurities in the insulating powder reacting with the ceramic blank during the sintering process. At the same time, controlling the particle size range of the insulating powder to 1μm to 100μm not only reduces the insulating powder due to too small particle size and too strong surface activity, which is easy to react with the ceramic blank and cause pitting on the finished ceramic substrate, but also does not cause pits on the surface of the ceramic substrate due to the excessive particle size of the insulating powder.
[0062] It can be understood that the purity of the isolation powder can be 99.99%, 99.995%, 99.999%, etc. ≥ 99.99% purity, and the particle size can be 1μm, 5μm, 10μm, 20μm, 30μm, 35μm, 40μm, 45μm, 50μm, 55μm, 60μm, 70μm, 80μm, 90μm, 100μm, etc., any value in the range of 1μm to 100μm.
[0063] In some embodiments, the insulating powder includes aluminum oxide, which is not easy to react with the ceramic green body to produce impurities.
[0064] In some embodiments, the thickness of a layer of insulating powder laid between any two layers of ceramic green bodies is 1 μm to 100 μm, and can be 1 μm, 5 μm, 10 μm, 20 μm, 30 μm, 40 μm, 50 μm, 60 μm, 70 μm, 80 μm, 90 μm, 100 μm, or any value in the range of 1 μm to 100 μm.
[0065] Exemplarily, in some embodiments, a process for preparing a ceramic substrate for reducing pinhole generation includes the following steps:
[0066] Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry, wherein the purity of the alumina powder is ≥ 99.9%;
[0067] Green billet molding: Pressing the slurry into a ceramic green billet;
[0068] Powder coating lamination: placing two or more layers of ceramic blanks on a firing plate, and laying a layer of insulating powder between any two of the ceramic blanks to obtain a powder-coated ceramic blank, wherein the purity of the insulating powder is ≥99.99%, and the particle size of the insulating powder is in the range of 1 μm to 100 μm;
[0069] Sintering: placing the powder-coated ceramic green body on the surface of the firing plate, heating the ceramic green body at a heating rate of 0.1°C / min to 0.5°C / min for sintering, and then cooling it at a cooling rate of 0.1°C / min to 0.5°C / min to obtain a ceramic substrate.
[0070] In some embodiments, the ceramic blank may be degreased before sintering to remove organic matter from the ceramic substrate blank, thereby reducing the generation of closed pores caused by residual organic matter and subsequently affecting the appearance of gray spots and other defects on the ceramic substrate.
[0071] In some embodiments of the degreasing treatment, the introduced degreasing gas includes air and / or nitrogen, and the air and / or nitrogen react with organic matter in the ceramic substrate blank to reduce the residual organic matter.
[0072] In some embodiments of the degreasing treatment, the degreasing gas is introduced at an air flow rate of 20L / min to 50L / min, and the ceramic substrate blank is heated at a heating rate of 0.2°C / min to 0.5°C / min to obtain a degreased ceramic substrate. For example, the air flow rate can be any value in the range of 20L / min to 50L / min, such as 20L / min, 25L / min, 30L / min, 35L / min, 40L / min, 45L / min, 50L / min, and the heating rate can be any value in the range of 0.2°C / min to 0.5°C / min, such as 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min. Under the above air flow rate and heating rate conditions, it is beneficial to discharge organic matter inside the ceramic substrate, reduce the generation of closed pores in the ceramic substrate blank during the sintering process due to the residual organic matter, and then affect the quality of the ceramic substrate, such as the appearance of defects such as gray spots.
[0073] In some embodiments of the degreasing treatment, the temperature is raised from room temperature 25°C to 30°C at a heating rate of 0.2°C / min to 0.5°C / min to 400°C to 800°C, and then kept warm. The holding time can be 4h to 6h. The degreasing treatment is carried out at 400°C to 800°C, which is conducive to promoting the discharge of organic matter and preventing excessive organic matter from remaining and causing gray spots on the ceramic substrate due to the formation of closed pores. In this embodiment, the temperature can be raised to any temperature in the range of 400°C to 800°C, such as 400°C, 450°C, 500°C, 550°C, 600°C, 650°C, 700°C, 750°C, 800°C, etc., and the holding time can be any value in the range of 4h to 6h, such as 4h, 4.5h, 5h, 5.5h, 6h, etc.
[0074] In some embodiments, a process for preparing a ceramic substrate for reducing pinhole generation includes the following steps:
[0075] Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry, wherein the purity of the alumina powder is ≥ 99.9%;
[0076] Green blank forming: pressing the slurry to form a ceramic green blank;
[0077] Degreasing: Degreasing the ceramic blank;
[0078] Sintering: The degreased ceramic blank is placed on the surface of a firing plate, heated at a heating rate of 0.1°C / min to 0.5°C / min for sintering, and then cooled at a cooling rate of 0.1°C / min to 0.5°C / min to obtain a ceramic substrate.
[0079] In some embodiments, the ceramic green body after powder coating and lamination may be degreased and then sintered.
[0080] In some embodiments, a sintering aid may be added to the step of mixing the alumina powder and the dispersant in the organic solvent for mixing and dispersing.
[0081] In this embodiment, a sintering aid may be added to the step of mixing the alumina powder and the dispersant in the organic solvent for mixing and dispersing.
[0082] The sintering step of the present invention can promote the shaping of the ceramic green body to obtain a ceramic substrate.
[0083] The heating rate in the sintering step is 0.1°C / min to 0.5°C / min. For example, it can be any value in the range of 0.1°C / min to 0.5°C / min, such as 0.1°C / min, 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min, etc. Under the above sintering heating rate conditions, it is beneficial to the sintering molding of the ceramic substrate, and the heating rate is slow, which is beneficial to promote the discharge of gas in the degreased ceramic green body and reduce the generation of pinholes in the finished ceramic substrate.
[0084] In some embodiments, the cooling rate is 0.1°C / min to 0.5°C / min. For example, it can be any value in the range of 0.1°C / min to 0.5°C / min, such as 0.1°C / min, 0.2°C / min, 0.3°C / min, 0.4°C / min, 0.5°C / min, etc. Under the above cooling rate conditions, the closed bubbles in the degreased ceramic green body can be caused to collapse in time, thereby reducing the generation of pinholes in the finished ceramic substrate.
[0085] In some embodiments, the temperature is lowered to 800° C. to 1000° C. at a temperature lowering rate of 0.1° C. / min to 0.5° C. / min.
[0086] In some implementations, after sintering, the temperature is kept at a high temperature for 2 to 4 hours.
[0087] In some embodiments, after the above-mentioned cooling is completed, the ceramic substrate can be naturally cooled to room temperature to obtain.
[0088] In some embodiments, the setter plate includes an alumina setter plate, which can reduce the problem of the setter plate reacting with the ceramic green body and affecting the quality of the finished ceramic substrate.
[0089] In some embodiments, the purity of the setter plate is ≥99.9%. The higher purity of the setter plate can reduce the pinhole defects in the ceramic substrate caused by the reaction of impurities in the ceramic blank and the setter plate.
[0090] In some embodiments of the sintering step, the sintering temperature ranges from 1450°C to 1600°C, and can be any value in the range of 1450°C to 1600°C, such as 1450°C, 1500°C, 1520°C, 1550°C, 1580°C, 1600°C, etc. Under the above sintering temperature conditions, it is beneficial to promote the sintering molding of the ceramic substrate.
[0091] In some embodiments, the purity of the alumina powder is ≥99.9%, and the heating rate and cooling rate in the sintering step are both 0.1°C / min to 0.5°C / min. This embodiment reduces the content of combustible impurities and volatile impurities in the raw materials by controlling the purity of the alumina powder, the raw material of the ceramic substrate, and reduces the pinholes in the ceramic substrate caused by the excessive generation of gas due to the combustible gas and volatile impurities during the sintering process. In addition, the sintering heating rate is controlled during the sintering process to promote the overflow of the gas, and the cooling rate is controlled to collapse the closed bubbles in time. Furthermore, by increasing the purity of the support plate so that the purity of the support plate is ≥99.9%, it is possible to reduce the pinhole defects in the ceramic substrate caused by the reaction of impurities in the ceramic blank and the support plate.
[0092] The ceramic substrate prepared by the method for preparing the ceramic substrate of the present invention as described above has good quality, a firm and stable structure, high density and fewer pinholes.
[0093] The technical solution of the present invention is further described in detail below in conjunction with specific embodiments. It should be understood that the following specific embodiments are only used to explain the present invention, and are not used to limit the present invention.
[0094] Example 1
[0095] Embodiment 1 A method for preparing a ceramic substrate comprises the following steps:
[0096] S10, preparing slurry: weighing 1000g of alumina powder with a particle size D50 of 0.6μm and a purity of 99.98%, dissolving it in a mixed solvent of 560g of ethyl acetate and 240g of ethanol, then adding 20g of dispersant triolein and 5g of sintering aid magnesium oxide with a particle size D50 of 0.5μm, mixing by ball milling for 24h, adding 100g of plasticizer dibutyl phthalate and 80g of binder polyvinyl butyral, and continuing mixing for 24h to obtain slurry;
[0097] S21, tape casting: casting the slurry into a green porcelain tape with a thickness of 60 μm;
[0098] S22, laminating isostatic pressing: laminating the green porcelain tape obtained after tape casting to a desired thickness, evacuating the green porcelain tape by a vacuum packaging machine, and after evacuation, placing the product in an isostatic pressing machine, setting the temperature to 60° C., the pressure to 80 MPa, and the holding time to 10 min to obtain a ceramic green body;
[0099] S23, degreasing: introducing a mixed gas of degreasing air and nitrogen at an air flow rate of 30 L / min, heating to 500° C. at a heating rate of 0.2° C. / min, and keeping the temperature for 2 hours to degrease the ceramic blank;
[0100] S40, sintering: placing the ceramic blank on the surface of an alumina support plate with a purity of 99.95%, heating the degreased ceramic blank to 1530°C at a heating rate of 0.1°C / min for sintering, then cooling the blank to 1000°C at a cooling rate of 0.1°C / min, and keeping the temperature for 4 hours to obtain a ceramic substrate.
[0101] Example 2 to Example 5
[0102] Examples 2 to 5 prepare ceramic substrates by referring to the preparation method of Example 1, except that the purity of alumina, sintering heating rate, sintering cooling rate, purity of the support plate, etc. of Examples 2 to 5 are different, as shown in Table 1 for details.
[0103] Comparative Example 1
[0104] Comparative Example 1 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the purity of the aluminum oxide powder used in Comparative Example 1 was 99.8%, as shown in Table 1.
[0105] Comparative Example 2
[0106] Comparative Example 2 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the purity of the aluminum oxide powder used in Comparative Example 2 was 99.0%, as shown in Table 1.
[0107] Comparative Example 3
[0108] Comparative Example 3 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the heating rate during the sintering process of Comparative Example 3 was 0.6° C. / min, as shown in Table 1 for details.
[0109] Comparative Example 4
[0110] Comparative Example 4 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the heating rate during the sintering process of Comparative Example 4 was 1° C. / min, as shown in Table 1 for details.
[0111] Comparative Example 5
[0112] Comparative Example 5 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the cooling rate during the sintering process of Comparative Example 5 was 1.5° C. / min, as shown in Table 1 for details.
[0113] Comparative Example 6
[0114] Comparative Example 6 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the cooling rate during the sintering process of Comparative Example 6 was 2° C. / min, as shown in Table 1 for details.
[0115] Comparative Example 7
[0116] Comparative Example 7 A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the purity of the setter plate used in Comparative Example 7 was 99.8%, as shown in Table 1 for details.
[0117] Comparative Example 8
[0118] Comparative Example 8: A ceramic substrate was prepared by referring to the preparation method of Example 1, except that the purity of the support plate used in Comparative Example 8 was 99.0%, as shown in Table 1.
[0119] Performance Testing
[0120] The number of gray spots on the surface of the ceramic substrates prepared in the examples and comparative examples was observed.
[0121] Table 1
[0122]
[0123] It can be known from Examples 1 to 5 and Comparative Examples 1 to 8 that Examples 1 to 5 improve the purity of alumina powder, reduce the content of combustible impurities and volatile impurities in alumina powder, and reduce the pinholes in the ceramic substrate caused by the excessive generation of gas due to the combustible gas and volatile impurities during the sintering process. In addition, during the sintering process, the sintering heating rate is controlled to 0.1°C / min to 0.5°C / min to promote the overflow of gas, and the cooling rate is controlled to 0.1°C / min to 0.5°C / min to prompt the bubbles to collapse in time to achieve the purpose of reducing the pinholes in the ceramic substrate. At the same time, the purity of the support plate can be improved to reduce the defects of pinholes in the ceramic substrate caused by the reaction of impurities in the ceramic blank and the support plate.
[0124] The purity of the alumina powder used in Comparative Example 1 is 99.8%, which is relatively low. The proportion of combustible impurities and volatile impurities in the alumina powder is relatively high. Excessive gas is easily generated during the sintering process, resulting in pinholes in the finished ceramic substrate. The number of pinholes is 8.
[0125] The purity of the alumina powder used in Comparative Example 2 is 99.0%, which is relatively low. The proportion of combustible impurities and volatile impurities in the alumina powder is relatively high. Excessive gas is easily generated during the sintering process, resulting in pinholes in the finished ceramic substrate. The number of pinholes is 15.
[0126] The heating rate of Comparative Example 3 during the sintering process is 0.6° C. / min. The heating rate is relatively high, and it is difficult to discharge the pores in the degreased ceramic green body, which easily leads to the appearance of pinholes in the finished ceramic substrate. The number of pinholes is 3.
[0127] In the comparative example 4, the heating rate during the sintering process is 1° C. / min. The heating rate is too high, and it is difficult to discharge the pores in the degreased ceramic green body, which easily leads to pinholes in the finished ceramic substrate. The number of pinholes is 7.
[0128] In the comparative example 5, the cooling rate during the sintering process was 1.5° C. / min, which was relatively high. The closed bubbles in the degreased green blank failed to collapse in time, resulting in 2 pinholes in the finished ceramic substrate.
[0129] In the comparative example 6, the cooling rate during the sintering process was 2° C. / min, which was relatively high. The closed bubbles in the degreased green blank failed to collapse in time, resulting in 7 pinholes in the finished ceramic substrate.
[0130] The purity of the setter plate used in Comparative Example 7 is 99.8%. The purity of the setter plate is relatively low, and it is easy to react with the degreased ceramic blank, thereby causing pinholes to appear in the finished ceramic substrate, and the number of pinholes is 8.
[0131] The purity of the setter plate used in Comparative Example 8 is 99.0%. The purity of the setter plate is relatively low, and it is easy to react with the degreased ceramic blank, thereby causing pinholes to appear in the finished ceramic substrate, and the number of pinholes is 16.
[0132] The above are only preferred embodiments of the present invention, and are not intended to limit the patent scope of the present invention. Any equivalent structure or equivalent process transformation made using the contents of the present invention specification and drawings, or directly or indirectly applied in other related technical fields, are also included in the patent protection scope of the present invention.
Claims
1. A process for preparing a ceramic substrate for reducing pinhole generation, characterized in that: The following steps are involved: Preparation of slurry: mixing alumina powder and a dispersant in an organic solvent, and then adding a plasticizer and a binder to obtain a slurry, wherein the purity of the alumina powder is ≥ 99.9%; Green blank forming: pressing the slurry to form a ceramic green blank; Sintering: placing the ceramic green blank on the surface of a sintering plate, heating the ceramic green blank at a heating rate of 0.1°C / min to 0.5°C / min for sintering, and then cooling the ceramic green blank at a cooling rate of 0.1°C / min to 0.5°C / min to obtain a ceramic substrate.
2. The process for preparing a ceramic substrate for reducing pinhole generation according to claim 1, characterized in that: The water content of the aluminum oxide powder is ≤0.1%.
3. The process for preparing a ceramic substrate for reducing pinhole generation according to claim 1, characterized in that: The particle size D50 of the aluminum oxide powder is 0.5 μm to 1.0 μm.
4. The process for preparing a ceramic substrate for reducing pinhole generation according to claim 1, characterized in that: The organic solvent includes alcohol compounds and ester compounds, wherein: The alcohol compound includes at least one of ethanol, propanol, isopropanol, ethylene glycol, n-butanol, and isobutanol; and / or the ester compound includes at least one of ethyl acetate, methyl acetate, propyl acetate, and butyl acetate.
5. The process for preparing a ceramic substrate for reducing pinhole generation according to claim 4, characterized in that: The organic solvent comprises an alcohol compound and an ester compound, and the mass ratio of the alcohol compound to the ester compound is (7-9):(1-3).
6. The process for preparing a ceramic substrate with reduced pinhole generation according to claim 1, characterized in that: The dispersant includes triolein; and / or, the plasticizer comprises at least one of dibutyl phthalate and polyethylene glycol; And / or, the binder comprises polyvinyl butyral.
7. The process for preparing a ceramic substrate with reduced pinhole generation according to claim 1, characterized in that: The purity of the aluminum oxide powder is 99.6% to 99.999%.
8. The process for preparing a ceramic substrate with reduced pinhole generation according to claim 1, characterized in that: The support plate comprises an alumina support plate; and / or the purity of the support plate is ≥99.9%.
9. The process for preparing a ceramic substrate with reduced pinhole generation according to claim 1, characterized in that: In the sintering step, the temperature is lowered to 800° C. to 1000° C. at a cooling rate of 0.1° C. / min to 0.5° C. / min.
10. A ceramic substrate prepared by the process for preparing a ceramic substrate with reduced pinhole generation according to any one of claims 1 to 9.
Citation Information
Patent Citations
Dumping and sintering process for 3D printing ceramic body
CN106316369A
Sintering method of dense oxide ceramic body
CN109020540A
High-purity ultrathin high-strength aluminum oxide ceramic substrate as well as preparation method and application thereof
CN114538900A
Alumina ceramic substrate and preparation method and application thereof
CN117700215A