Method for improving hydrophilicity of carbon fiber precursor spinning solution

Ammonium itaconic acid is generated by ammonia and itaconic acid, and combined with sodium thiocyanate, the hydrophilicity of the acrylonitrile-itaconic acid binary copolymer is improved, and the hydrophilicity regulation of carbon fiber protofilament spinning solution is solved The problem has improved the solidification process of the spinning liquid and the structural homogeneity of carbon fibers.

CN118994475APending Publication Date: 2024-11-22ZHONGFU SHENYING CARBON FIBER +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411114957.9
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-14
Publication Date
2024-11-22

AI Technical Summary

Technical Problem

The hydrophobic properties of the polyacrylonitrile molecular chain and the extrusion swelling effect in spinning lead to differences in the radial structure of carbon fiber protofilament. The prior art has limitations in regulating the temperature and composition of the solidification bath, making it difficult to effectively improve the structural homogeneity of the fiber.

Method used

Ammonia gas and itaconic acid are used to generate ammonium itaconic acid, combined with sodium thiocyanate, to improve the hydrophilicity of acrylonitrile-itaconic acid binary copolymer through chemical reaction, and regulate the solidification phase separation process of the spinning liquid to form Carbon fiber raw silk with good hydrophilicity.

Benefits of technology

The hydrophilicity of the carbon fiber proto-filament spinning solution is realized, the solidification process of the spinning liquid is improved, and the quality and structural homogeneity of the carbon fiber precursor are improved.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses a method for improving hydrophilicity of a carbon fiber precursor spinning solution. The method comprises the following steps: firstly, introducing a dimethyl sulfoxide solution of azodiisobutyronitrile, itaconic acid and acrylonitrile into a mixing zone in a tubular static mixer, uniformly mixing, then feeding into a heating zone, raising the temperature to a set temperature, then feeding into a reaction zone for polymerization reaction, then feeding into a full-mixing type polymerization kettle for continuous reaction, and finally discharging to obtain a finished product. Ammonia gas is introduced into the formed acrylonitrile-itaconic acid binary copolymer solution, a NaSCN solution is added, and a spinning stock solution is formed after aging, demonomerisation and filtration. Ammonia gas and sodium thiocyanate are adopted to perform hydrophilic modification on the acrylonitrile-itaconic acid binary copolymer, so that the hydrophilicity of the carbon fiber precursor spinning solution can be further improved, the double-diffusion speed and the solidification phase separation process of the spinning solution in the solidification process are effectively improved, and the radial structure homogeneity of the polyacrylonitrile fiber is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of polyacrylonitrile fiber modification and relates to a method for improving the hydrophilicity of a carbon fiber precursor spinning solution. Background Art

[0002] Acrylonitrile / itaconic acid copolymer is an important precursor material for the preparation of high-performance carbon fiber. Coagulation spinning of copolymer solution is the most critical step in the preparation of carbon fiber precursor, and the control of coagulation phase separation directly affects the structural homogeneity of the fiber. The hydrophobic properties of polyacrylonitrile (PAN) molecular chains and the extrusion swelling effect during spinning lead to serious radial structural differences in coagulated fibers, which is an important factor affecting the high performance of carbon fiber. Although the coagulation phase separation process can be adjusted by regulating factors such as the coagulation bath temperature and the composition of the coagulation bath, this approach has certain limitations. Hydrophilic modification of the polymer and slowing down the coagulation phase transition rate of acrylonitrile polymer in a water-based coagulant system are the main means to regulate the radial structural homogeneity of polyacrylonitrile fibers.

[0003] Ammonia can modify the hydrophilicity of acrylonitrile copolymers by acting on the comonomer itaconic acid. Ammonia can react chemically with itaconic acid to generate ammonium itaconate with better hydrophilicity, thereby improving the hydrophilicity of the copolymer. However, there are two critical points in the contact angle between ammonia solution and acrylonitrile copolymers, that is, when the concentration of ammonia is not enough, the hydrophilicity of the copolymer cannot be improved. When the concentration of ammonia is too high, the hydrophilicity modification effect is no longer improved. Summary of the invention

[0004] The object of the present invention is to provide a method for improving the hydrophilicity of a carbon fiber precursor spinning solution.

[0005] The technical solution for achieving the purpose of the present invention is as follows:

[0006] A method for improving the hydrophilicity of a carbon fiber precursor spinning solution comprises the following steps:

[0007] A dimethyl sulfoxide solution of azobisisobutyronitrile, itaconic acid and acrylonitrile is introduced into the mixing zone of a tubular static mixer, mixed evenly and then enters the heating zone, and then enters the reaction zone after being heated to the set temperature. After the polymerization reaction is carried out at 50-57°C for 40-60 minutes, it is sent to a fully mixed polymerization kettle, reacted at 45-55°C for 18-30 hours, and then ammonia is introduced into the formed acrylonitrile-itaconic acid binary copolymer solution at a molar ratio of itaconic acid to ammonia of 1:1.2, and then NaSCN solution is added at a mass ratio of NaSCN to itaconic acid of 5-15:100, and a spinning solution is formed after aging, de-sing and filtration.

[0008] Furthermore, the solid content of the acrylonitrile-itaconic acid copolymer solution is 15-20%, preferably 17%.

[0009] Furthermore, the mass ratio of acrylonitrile to itaconic acid is 95-99:1-5, preferably 98:2.

[0010] Furthermore, the temperature of the mixing zone is 35-45°C.

[0011] Furthermore, the mass ratio of NaSCN to itaconic acid is 10:100.

[0012] Furthermore, the mass concentration of the NaSCN solution is 5%.

[0013] Compared with the prior art, the present invention has the following advantages:

[0014] The present invention uses ammonia and sodium thiocyanate to modify the hydrophilicity of acrylonitrile-itaconic acid binary copolymer, ammonia and itaconic acid produce a chemical reaction to generate ammonium itaconate, so that the carbon fiber precursor has good hydrophilicity but there is a critical concentration, and sodium thiocyanate can achieve adjustable hydrophilicity and significant modification effect by complexing with cyano group. The present invention achieves controllable adjustment of the hydrophilicity of the precursor spinning solution by mixing ammonia and sodium thiocyanate, improves the double diffusion speed and coagulation phase separation process of the spinning solution during the coagulation process, and is conducive to improving the quality of the carbon fiber precursor. DETAILED DESCRIPTION

[0015] The present invention is further described in detail below in conjunction with specific embodiments.

[0016] In the following examples and comparative examples, the film samples were prepared as follows:

[0017] The spinning solution was coated on the edge of a flat glass plate, and a film was scraped out on the glass plate with a film scraper. The glass plate with the spinning solution film was coagulated in a 25% DMSO / water coagulation bath for 40 minutes. After the coagulation was completed, it was rinsed three times with deionized water and a film sample was obtained after it was fully dried.

[0018] Example 1

[0019] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%. Ammonia is passed into the solution according to the molar ratio of itaconic acid to ammonia of 1:1.2, and then a NaSCN solution of the same mass as itaconic acid is added, and the mass concentration of the NaSCN solution is 5%. Finally, after aging, stripping and filtering, a spinning solution is formed.

[0020] The thickness of the film sample was measured to be 93 μm, and the water contact angle of the film sample was measured to be 38.2° by a static contact angle meter.

[0021] Example 2

[0022] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%. Ammonia is passed into the solution according to the molar ratio of itaconic acid to ammonia of 1:1.2, and then a NaSCN solution with a mass of 2 times the mass of itaconic acid is added, and the mass concentration of the NaSCN solution is 5%. Finally, after aging, stripping and filtering, a spinning solution is formed.

[0023] The thickness of the film sample was measured to be 107 μm, and the water contact angle of the film sample was measured to be 32.6° by a static contact angle meter.

[0024] Example 3

[0025] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%. Ammonia is passed into the solution according to the molar ratio of itaconic acid to ammonia of 1:1.2, and then a NaSCN solution of 3 times the mass of itaconic acid is added, and the mass concentration of the NaSCN solution is 5%. Finally, after aging, stripping and filtering, a spinning solution is formed.

[0026] The thickness of the film sample was measured to be 86 μm, and the water contact angle of the film sample was measured to be 36.9° by a static contact angle meter.

[0027] Comparative Example 1

[0028] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%, and finally after aging, de-sing and filtering, it forms a spinning solution.

[0029] The thickness of the film sample was measured to be 93 μm, and the water contact angle of the film sample was measured to be 44.8° by a static contact angle meter.

[0030] Comparative Example 2

[0031] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%. Ammonia is passed into the solution according to the molar ratio of itaconic acid to ammonia of 1:1.2, and finally, after aging, stripping and filtering, a spinning solution is formed.

[0032] The thickness of the film sample was measured to be 114 μm, and the water contact angle of the film was measured by a static contact angle meter to be 39.6°.

[0033] Comparative Example 3

[0034] According to the mass ratio of acrylonitrile to itaconic acid of 98:2, the molar ratio of initiator azobisisobutyronitrile to acrylonitrile of 0.3%:1, the dimethyl sulfoxide solution of acrylonitrile, itaconic acid and azobisisobutyronitrile is passed into the mixing zone in the tubular static mixer, and the temperature of the mixing zone is controlled at 35°C. After being mixed evenly, it enters the heating zone, and after rising to 50°C, it is sent to the reaction zone for polymerization reaction for 40 minutes, and then sent to the fully mixed polymerization kettle, and reacted at 50°C for 20 hours to obtain an acrylonitrile-itaconic acid binary copolymer solution with a solid content of 17%, and then a NaSCN solution of the same mass as itaconic acid is added, and the mass concentration of the NaSCN solution is 5%. Finally, after aging, de-sing and filtration, a spinning solution is formed.

[0035] The thickness of the film sample was measured to be 137 μm, and the water contact angle of the film sample was measured to be 41.2° by a static contact angle meter.

Claims

1. A method for improving the hydrophilicity of a carbon fiber precursor spinning solution, characterized in that: The following steps are involved: A dimethyl sulfoxide solution of azobisisobutyronitrile, itaconic acid and acrylonitrile is introduced into the mixing zone of a tubular static mixer, mixed evenly and then enters the heating zone, and then enters the reaction zone after being heated to the set temperature. After the polymerization reaction is carried out at 50-57°C for 40-60 minutes, it is sent to a fully mixed polymerization kettle, reacted at 45-55°C for 18-30 hours, and then ammonia is introduced into the formed acrylonitrile-itaconic acid binary copolymer solution at a molar ratio of itaconic acid to ammonia of 1:1.2, and then NaSCN solution is added at a mass ratio of NaSCN to itaconic acid of 5-15:100, and a spinning solution is formed after aging, de-sing and filtration.

2. The method according to claim 1, characterized in that The solid content of the acrylonitrile-itaconic acid copolymer solution is 15-20%.

3. The method according to claim 1, characterized in that The solid content of the acrylonitrile-itaconic acid copolymer solution is 17%.

4. The method according to claim 1, characterized in that The mass ratio of acrylonitrile to itaconic acid is 95~99:1~5.

5. The method according to claim 1, characterized in that The mass ratio of acrylonitrile to itaconic acid is 98:

2.

6. The method according to claim 1, characterized in that The temperature in the mixing zone is 35~45℃.

7. The method according to claim 1, characterized in that The mass ratio of NaSCN to itaconic acid is 10:

100.

8. The method according to claim 1, characterized in that The mass concentration of NaSCN solution is 5%.